Chinese JoineryChinese Joinery
Wood

Oak wood

Swamp white oak is the hardest oak in the Handbook at 1,620 lbf1; southern red oak is the softest at 1,060 lbf2. Live oak has no 12% Janka value, so it is not in that ranking. The Handbook splits oaks into a red oak group and a white oak group3.

Red oak group

Specific gravity is 12% MC volume basis. Janka, MOR, and MOE are 12% moisture values. A blank cell is not printed in the Handbook.

Pin oak1,51020.63214,00021.7329.550.003386
Cherrybark oak1,48020.68218,10022.282
Willow oak1,46010.69114,50011.919.650.003487
Scarlet oak1,40020.67217,40021.91210.850.003886
Northern red oak1,29020.63214,30021.8228.650.003046
Black oak1,21020.61213,90021.64211.150.0046
Laurel oak1,21020.63212,60021.6929.950.003487
Water oak1,19010.63115,40012.0219.850.003487
Southern red oak1,06020.59210,90021.49211.350.00407, calculated8

Movement coefficients for willow oak, laurel oak, and water oak are the Handbook’s group row “Red oak: water, laurel, willow”, printed once for the whole group rather than measured separately for each species.

White oak group

Specific gravity is 12% MC volume basis. Janka, MOR, and MOE are 12% moisture values. A blank cell is not printed in the Handbook.

Swamp white oak1,62010.72117,70012.051
Bur oak1,37010.64110,30011.0318.850.003126
White oak1,36010.68115,20011.78110.550.003766
Post oak1,36010.67113,20011.5119.850.0035, calculated8
Swamp chestnut oak1,24010.67113,90011.77110.850.00388, calculated8
Overcup oak1,19010.63112,60011.42112.750.004626
Chestnut oak1,13010.66113,30011.59110.850.00388, calculated8
Live oak0.88118,40011.9819.550.003386

In the strength tables the live oak row is Oak, white/Live1. Chapter 2 compares tropical oaks with the oaks of the United States, especially live oak4.

Pages

Questions

Which oak is hardest?
Swamp white oak at 1,620 lbf1, among the oak rows that have a 12% Janka value.
Which oak is softest?
Southern red oak at 1,060 lbf2.
Is oak a hardwood?
Yes. All 17 oak rows in this list are hardwoods9.

References

  • 1. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-11
  • 2. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-10
  • 3. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-9
  • 4. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-31
  • 5. USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8
  • 6. USDA Wood Handbook (FPL-GTR-282), Table 13-5, p. 13-17
  • 7. USDA Wood Handbook (FPL-GTR-282), Table 13-5, p. 13-17 (row “Red oak: water, laurel, willow”)
  • 8. Calculated with Wood Handbook Eq. 13-2 (p. 13-16) from Table 4-3 (p. 4-8)
  • 9. Calculated by counting rows in USDA Wood Handbook (FPL-GTR-282) Tables 5-3 and 5-5.