Birch vs Oak wood
Northern red oak (red oak group) is harder than yellow birch but weaker in bending and less stiff: 1,2901 vs 1,2602 lbf, 2% harder3. White oak (white oak group) is harder than yellow birch but weaker in bending and less stiff: 1,3604 vs 1,2602 lbf, 8% harder3. Movement across a flat-sawn board is split, from least to most: northern red oak CT 0.003045, yellow birch CT 0.003385, and white oak CT 0.003765. Northern red oak and white oak are denser (specific gravity 0.631 and 0.684 vs 0.622, 12% MC volume basis).
Side by side
| Property | Birch (yellow birch) | Northern red oak (red oak group) | White oak (white oak group) |
|---|---|---|---|
| Janka hardness, 12% MC | 1,260 lbf2; 5,600 N6 | 1,290 lbf1; 5,700 N7 | 1,360 lbf4; 6,000 N8 |
| Janka hardness, green | 780 lbf2 | 1,000 lbf1 | 1,060 lbf4 |
| Specific gravity, 12% MC volume basis | 0.622 | 0.631 | 0.684 |
| Bending strength (MOR), 12% MC | 16,600 psi2; 114,000 kPa6 | 14,300 psi1; 99,000 kPa7 | 15,200 psi4; 105,000 kPa8 |
| Stiffness (MOE), 12% MC | 2.01 × 106 psi2; 13,900 MPa6 | 1.82 × 106 psi1; 12,500 MPa7 | 1.78 × 106 psi4; 12,300 MPa8 |
| Shrinkage, green to oven-dry | radial 7.3%, tangential 9.5%, volumetric 16.8%9 | radial 4%, tangential 8.6%, volumetric 13.7%9 | radial 5.6%, tangential 10.5%, volumetric 16.3%9 |
| T/R ratio (tangential ÷ radial) | 1.30, calculated10 | 2.15, calculated10 | 1.88, calculated10 |
| Movement coefficients | CR 0.00256; CT 0.003385 | CR 0.00137; CT 0.003045 | CR 0.00194; CT 0.003765 |
Which to use
For a tabletop that must resist dents, white oak (white oak group) is the harder wood at 1,360 lbf4, against yellow birch at 1,260 lbf2.
For a wide flat-sawn panel, northern red oak (red oak group) moves less (CT 0.003045, against white oak at 0.003765).
Related
Questions
- Is birch harder than oak?
- No. Northern red oak (red oak group) at 1,290 lbf1 and white oak (white oak group) at 1,360 lbf4 are harder than yellow birch at 1,260 lbf2.
- Which moves more, birch or oak?
- It depends on the row. Yellow birch CT 0.003385; northern red oak (red oak group) and white oak (white oak group) CT 0.003045 and CT 0.003765.
References
- 1. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-10
- 2. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-9
- 3. Calculated from the two 12% Janka values: the difference divided by the lower value.
- 4. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-11
- 5. USDA Wood Handbook (FPL-GTR-282), Table 13-5, p. 13-17
- 6. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-4
- 7. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-5
- 8. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-6
- 9. USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8
- 10. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8).