Chinese JoineryChinese Joinery
Wood

Red oak (northern red oak) wood

Red oak (northern red oak, Quercus rubra) is a medium-hard hardwood2: 1,290 lbf1 on the Janka side-hardness test at 12% moisture, below white oak (1,360 lbf3) and above black walnut (1,010 lbf3).

It is moderately stiff4, and it moves about 0.30%5 across the width of a flat-sawn board for each 1% change in moisture content.

Key numbers

PropertyNorthern red oak
Janka hardness, 12% MC1,290 lbf1; 5,700 N6
Janka hardness, green1,000 lbf1
Specific gravity, 12% MC volume basis0.631
Bending strength (MOR), 12% MC14,300 psi1; 99,000 kPa6
Stiffness (MOE), 12% MC1.82 × 106 psi1; 12,500 MPa6
Shrinkage, green to oven-dryradial 4%, tangential 8.6%, volumetric 13.7%7
T/R ratio (tangential ÷ radial)2.15, calculated8
Movement coefficientsCR 0.00137; CT 0.003045

How hard is red oak (northern red oak)?

01,0002,0003,0004,000northern red oak 1,290 lbf

Ticks are the anchor woods, from eastern white pine to ipe; the scale is in lbf. See northern red oak on the Janka chart.

How much does it move?

A 10-inch flat-sawn northern red oak board going from 6% to 10% moisture content, the range the Handbook recommends for individual pieces of interior woodwork in most of the United States10, widens by 0.122 in9. A quartersawn board widens by 0.055 in9.

The coefficients apply from 6% to 14% moisture content11.

Try your own board in the wood movement calculator.

What it's used for

Northern red oak is a principal species of the red oak group. The sapwood is nearly white and the heartwood is brown with a tinge of red; quartersawn oak shows broad, conspicuous rays. The lumber is remanufactured into flooring, furniture, millwork, boxes, pallets, crates, and handles, and the group is also cut for ties, mine timbers, fence posts, veneer, and fuelwood.12

Compare with

Questions

Is red oak a hardwood?
Yes. Red oak is a hardwood13. In the Handbook, hardwood means a broad-leaved angiosperm, not a wood that is necessarily hard. Specific gravity on a 12% MC volume basis is 0.631.
Is red oak harder than white oak?
Red oak is softer than white oak: 1,290 lbf1 versus 1,360 lbf3, both at 12% moisture.
How much does red oak shrink?
From green to oven-dry, tangential shrinkage is 8.6% and radial shrinkage is 4%7. The T/R ratio is 2.15, calculated8.

References

  • 1. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-10
  • 2. Calculated from the 12% moisture Janka side-hardness values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 3. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-11
  • 4. Calculated from the 12% moisture modulus of elasticity values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 5. USDA Wood Handbook (FPL-GTR-282), Table 13-5, p. 13-17
  • 6. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-5
  • 7. USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8
  • 8. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8).
  • 9. Calculated with Wood Handbook Eq. 13-3 (p. 13-16): 10 in × the coefficient × 4 percentage points. Tangential coefficient 0.00304; radial coefficient 0.00137.
  • 10. USDA Wood Handbook (FPL-GTR-282), Table 13-2, p. 13-5
  • 11. USDA Wood Handbook (FPL-GTR-282), ch. 13, p. 13-16
  • 12. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-9
  • 13. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-2