Cedar vs Oak wood
Western redcedar is softer, weaker in bending and less stiff than northern red oak (red oak group) and white oak (white oak group): 3501 vs 1,2902 and 1,3603 lbf. Eastern redcedar is weaker in bending and less stiff than both. Eastern redcedar has no 12% pound-force Janka value in the Handbook, only 4,000 N4, so it is not given a percent difference. Western redcedar and eastern redcedar move less across a flat-sawn board (CT 0.002345 and 0.001625 vs 0.003045 and 0.003765). Northern red oak and white oak are denser (specific gravity 0.632 and 0.683 vs 0.321 and 0.473, 12% MC volume basis).
Side by side
| Property | Western redcedar | Eastern redcedar | Northern red oak (red oak group) | White oak (white oak group) |
|---|---|---|---|---|
| Janka hardness, 12% MC | 350 lbf1; 1,600 N6 | 4,000 N4; ≈ 900 lbf, calculated7 | 1,290 lbf2; 5,700 N8 | 1,360 lbf3; 6,000 N4 |
| Janka hardness, green | 260 lbf1 | 650 lbf3 | 1,000 lbf2 | 1,060 lbf3 |
| Specific gravity, 12% MC volume basis | 0.321 | 0.473 | 0.632 | 0.683 |
| Bending strength (MOR), 12% MC | 7,500 psi1; 51,700 kPa6 | 8,800 psi3; 61,000 kPa4 | 14,300 psi2; 99,000 kPa8 | 15,200 psi3; 105,000 kPa4 |
| Stiffness (MOE), 12% MC | 1.11 × 106 psi1; 7,700 MPa6 | 0.88 × 106 psi3; 6,100 MPa4 | 1.82 × 106 psi2; 12,500 MPa8 | 1.78 × 106 psi3; 12,300 MPa4 |
| Shrinkage, green to oven-dry | radial 2.4%, tangential 5%, volumetric 6.8%9 | radial 3.1%, tangential 4.7%, volumetric 7.8%9 | radial 4%, tangential 8.6%, volumetric 13.7%9 | radial 5.6%, tangential 10.5%, volumetric 16.3%9 |
| T/R ratio (tangential ÷ radial) | 2.08, calculated10 | 1.52, calculated10 | 2.15, calculated10 | 1.88, calculated10 |
| Movement coefficients | CR 0.00111; CT 0.002345 | CR 0.00106; CT 0.001625 | CR 0.00137; CT 0.003045 | CR 0.00194; CT 0.003765 |
Which to use
For a tabletop that must resist dents, white oak (white oak group) is the harder wood at 1,360 lbf3, against western redcedar at 350 lbf1.
For a wide flat-sawn panel, eastern redcedar moves less (CT 0.001625, against white oak at 0.003765).
Related
Questions
- Is cedar harder than oak?
- No. Northern red oak (red oak group) at 1,290 lbf2 and white oak (white oak group) at 1,360 lbf3 are harder than western redcedar at 350 lbf1.
- Which moves more, cedar or oak?
- Northern red oak (red oak group) and white oak (white oak group) move more than western redcedar and eastern redcedar across a flat-sawn board (CT 0.003045 and CT 0.003765 vs CT 0.002345 and CT 0.001625).
References
- 1. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-12
- 2. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-10
- 3. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-11
- 4. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-6
- 5. USDA Wood Handbook (FPL-GTR-282), Table 13-5, p. 13-17
- 6. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-7
- 7. Calculated from 4,000 N in USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-6, using 1 lbf = 4.448 N (≈ 900 lbf). Not used in the 12% ranking.
- 8. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-5
- 9. USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8
- 10. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8).