Chinese JoineryChinese Joinery
Wood

Black oak wood

Black oak is a medium-hard hardwood2: 1,210 lbf1 on the Janka side-hardness test at 12% moisture, below northern red oak (1,290 lbf1) and above black walnut (1,010 lbf3).

It is flexible4, and it moves about 0.40%5 across the width of a flat-sawn board for each 1% change in moisture content.

Key numbers

PropertyBlack oak
Janka hardness, 12% MC1,210 lbf1; 5,400 N6
Janka hardness, green1,060 lbf1
Specific gravity, 12% MC volume basis0.611
Bending strength (MOR), 12% MC13,900 psi1; 96,000 kPa6
Stiffness (MOE), 12% MC1.64 × 106 psi1; 11,300 MPa6
Shrinkage, green to oven-dryradial 4.4%, tangential 11.1%, volumetric 15.1%7
T/R ratio (tangential ÷ radial)2.52, calculated8
Movement coefficientsCR 0.00151; CT 0.0045

How hard is black oak?

01,0002,0003,0004,000black oak 1,210 lbf

Ticks are the anchor woods, from eastern white pine to ipe; the scale is in lbf. See black oak on the Janka chart.

How much does it move?

A 10-inch flat-sawn black oak board going from 6% to 10% moisture content, the range the Handbook recommends for individual pieces of interior woodwork in most of the United States10, widens by 0.160 in9. A quartersawn board widens by 0.060 in9.

The coefficients apply from 6% to 14% moisture content11.

Try your own board in the wood movement calculator.

What it's used for

Black oak is a principal species of the red oak group. The sapwood is nearly white and the heartwood is brown with a tinge of red; quartersawn oak shows broad, conspicuous rays. Red oak lumber is used for flooring, furniture, millwork, boxes, pallets, crates, and handles, and also for ties, mine timbers, fence posts, veneer, and fuelwood.12

Compare with

Questions

Is black oak a hardwood?
Yes. Black oak is a hardwood13. In the Handbook, hardwood means a broad-leaved angiosperm, not a wood that is necessarily hard. Specific gravity on a 12% MC volume basis is 0.611.
Is black oak harder than northern red oak?
Black oak is softer than northern red oak: 1,210 lbf1 versus 1,290 lbf1, both at 12% moisture.
How much does black oak shrink?
From green to oven-dry, tangential shrinkage is 11.1% and radial shrinkage is 4.4%7. The T/R ratio is 2.52, calculated8.

References

  • 1. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-10
  • 2. Calculated from the 12% moisture Janka side-hardness values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 3. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-11
  • 4. Calculated from the 12% moisture modulus of elasticity values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 5. USDA Wood Handbook (FPL-GTR-282), Table 13-5, p. 13-17
  • 6. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-5
  • 7. USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8
  • 8. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8).
  • 9. Calculated with Wood Handbook Eq. 13-3 (p. 13-16): 10 in × the coefficient × 4 percentage points. Tangential coefficient 0.004; radial coefficient 0.00151.
  • 10. USDA Wood Handbook (FPL-GTR-282), Table 13-2, p. 13-5
  • 11. USDA Wood Handbook (FPL-GTR-282), ch. 13, p. 13-16
  • 12. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-9
  • 13. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-2