Oak vs Pine wood
Northern red oak (red oak group) is harder than eastern white pine and longleaf pine (southern yellow pine), and falls between them in bending strength and stiffness: 1,2901 vs 3802 and 8702 lbf, 48% to 239% harder3. White oak (white oak group) is harder and stronger in bending than both, and falls between them in stiffness: 1,3604 vs 3802 and 8702 lbf, 56% to 258% harder3. Eastern white pine and longleaf pine move less across a flat-sawn board (CT 0.002125 and 0.002485 vs 0.003045 and 0.003765). Northern red oak and white oak are denser (specific gravity 0.631 and 0.684 vs 0.352 and 0.592, 12% MC volume basis).
Side by side
| Property | Northern red oak (red oak group) | White oak (white oak group) | Eastern white pine | Longleaf pine (southern yellow pine) |
|---|---|---|---|---|
| Janka hardness, 12% MC | 1,290 lbf1; 5,700 N6 | 1,360 lbf4; 6,000 N7 | 380 lbf2; 1,700 N8 | 870 lbf2; 3,900 N8 |
| Janka hardness, green | 1,000 lbf1 | 1,060 lbf4 | 290 lbf2 | 590 lbf2 |
| Specific gravity, 12% MC volume basis | 0.631 | 0.684 | 0.352 | 0.592 |
| Bending strength (MOR), 12% MC | 14,300 psi1; 99,000 kPa6 | 15,200 psi4; 105,000 kPa7 | 8,600 psi2; 59,000 kPa8 | 14,500 psi2; 100,000 kPa8 |
| Stiffness (MOE), 12% MC | 1.82 × 106 psi1; 12,500 MPa6 | 1.78 × 106 psi4; 12,300 MPa7 | 1.24 × 106 psi2; 8,500 MPa8 | 1.98 × 106 psi2; 13,700 MPa8 |
| Shrinkage, green to oven-dry | radial 4%, tangential 8.6%, volumetric 13.7%9 | radial 5.6%, tangential 10.5%, volumetric 16.3%9 | radial 2.1%, tangential 6.1%, volumetric 8.2%9 | radial 5.1%, tangential 7.5%, volumetric 12.2%9 |
| T/R ratio (tangential ÷ radial) | 2.15, calculated10 | 1.88, calculated10 | 2.90, calculated10 | 1.47, calculated10 |
| Movement coefficients | CR 0.00137; CT 0.003045 | CR 0.00194; CT 0.003765 | CR 0.00071; CT 0.002125 | CR 0.00137; CT 0.002485 |
Which to use
For a tabletop that must resist dents, white oak (white oak group) is the harder wood at 1,360 lbf4, against eastern white pine at 380 lbf2.
For a wide flat-sawn panel, eastern white pine moves less (CT 0.002125, against white oak at 0.003765).
Related
Questions
- Is oak harder than pine?
- Yes. Northern red oak (red oak group) at 1,290 lbf1 and white oak (white oak group) at 1,360 lbf4 are harder than eastern white pine at 380 lbf2 and longleaf pine (southern yellow pine) at 870 lbf2.
- Which moves more, oak or pine?
- Northern red oak (red oak group) and white oak (white oak group) move more than eastern white pine and longleaf pine (southern yellow pine) across a flat-sawn board (CT 0.003045 and CT 0.003765 vs CT 0.002125 and CT 0.002485).
References
- 1. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-10
- 2. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-12
- 3. Calculated from the two 12% Janka values: the difference divided by the lower value.
- 4. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-11
- 5. USDA Wood Handbook (FPL-GTR-282), Table 13-5, p. 13-17
- 6. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-5
- 7. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-6
- 8. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-7
- 9. USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8
- 10. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8).