Chinese JoineryChinese Joinery
Wood

Oak vs Walnut wood

Northern red oak (red oak group) is harder and stiffer than black walnut but weaker in bending: 1,2901 vs 1,0102 lbf, 28% harder3. White oak (white oak group) is harder, stronger in bending and stiffer than black walnut: 1,3602 vs 1,0102 lbf, 35% harder3. Black walnut moves less across a flat-sawn board (CT 0.002744 vs 0.003044 and 0.003764). Northern red oak and white oak are denser (specific gravity 0.631 and 0.682 vs 0.552, 12% MC volume basis).

Side by side

PropertyNorthern red oak (red oak group)White oak (white oak group)Black walnut
Janka hardness, 12% MC1,290 lbf1; 5,700 N51,360 lbf2; 6,000 N61,010 lbf2; 4,500 N6
Janka hardness, green1,000 lbf11,060 lbf2900 lbf2
Specific gravity, 12% MC volume basis0.6310.6820.552
Bending strength (MOR), 12% MC14,300 psi1; 99,000 kPa515,200 psi2; 105,000 kPa614,600 psi2; 101,000 kPa6
Stiffness (MOE), 12% MC1.82 × 106 psi1; 12,500 MPa51.78 × 106 psi2; 12,300 MPa61.68 × 106 psi2; 11,600 MPa6
Shrinkage, green to oven-dryradial 4%, tangential 8.6%, volumetric 13.7%7radial 5.6%, tangential 10.5%, volumetric 16.3%7radial 5.5%, tangential 7.8%, volumetric 12.8%7
T/R ratio (tangential ÷ radial)2.15, calculated81.88, calculated81.42, calculated8
Movement coefficientsCR 0.00137; CT 0.003044CR 0.00194; CT 0.003764CR 0.0019; CT 0.002744

Which to use

For a tabletop that must resist dents, white oak (white oak group) is the harder wood at 1,360 lbf2, against black walnut at 1,010 lbf2.

For a wide flat-sawn panel, black walnut moves less (CT 0.002744, against white oak at 0.003764).

Related

Questions

Is oak harder than walnut?
Yes. Northern red oak (red oak group) at 1,290 lbf1 and white oak (white oak group) at 1,360 lbf2 are harder than black walnut at 1,010 lbf2.
Which moves more, oak or walnut?
Northern red oak (red oak group) and white oak (white oak group) move more than black walnut across a flat-sawn board (CT 0.003044 and CT 0.003764 vs CT 0.002744).

References

  • 1. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-10
  • 2. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-11
  • 3. Calculated from the two 12% Janka values: the difference divided by the lower value.
  • 4. USDA Wood Handbook (FPL-GTR-282), Table 13-5, p. 13-17
  • 5. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-5
  • 6. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-6
  • 7. USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8
  • 8. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8).