Northern red oak (red oak group) is harder, stronger in bending and stiffer than yellow-poplar: 1,2901 vs 5402 lbf, 139% harder3. White oak (white oak group) is harder, stronger in bending and stiffer than yellow-poplar: 1,3602 vs 5402 lbf, 152% harder3. Yellow-poplar moves less across a flat-sawn board (CT 0.002894 vs 0.003044 and 0.003764). Northern red oak and white oak are denser (specific gravity 0.631 and 0.682 vs 0.422, 12% MC volume basis).
Side by side
| Property | Northern red oak (red oak group) | White oak (white oak group) | Poplar (yellow-poplar) |
|---|---|---|---|
| Janka hardness, 12% MC | 1,290 lbf1; 5,700 N5 | 1,360 lbf2; 6,000 N6 | 540 lbf2; 2,400 N6 |
| Janka hardness, green | 1,000 lbf1 | 1,060 lbf2 | 440 lbf2 |
| Specific gravity, 12% MC volume basis | 0.631 | 0.682 | 0.422 |
| Bending strength (MOR), 12% MC | 14,300 psi1; 99,000 kPa5 | 15,200 psi2; 105,000 kPa6 | 10,100 psi2; 70,000 kPa6 |
| Stiffness (MOE), 12% MC | 1.82 × 106 psi1; 12,500 MPa5 | 1.78 × 106 psi2; 12,300 MPa6 | 1.58 × 106 psi2; 10,900 MPa6 |
| Shrinkage, green to oven-dry | radial 4%, tangential 8.6%, volumetric 13.7%7 | radial 5.6%, tangential 10.5%, volumetric 16.3%7 | radial 4.6%, tangential 8.2%, volumetric 12.7%7 |
| T/R ratio (tangential ÷ radial) | 2.15, calculated8 | 1.88, calculated8 | 1.78, calculated8 |
| Movement coefficients | CR 0.00137; CT 0.003044 | CR 0.00194; CT 0.003764 | CR 0.00158; CT 0.002894 |
Which to use
For a tabletop that must resist dents, white oak (white oak group) is the harder wood at 1,360 lbf2, against yellow-poplar at 540 lbf2.
For a wide flat-sawn panel, yellow-poplar moves less (CT 0.002894, against white oak at 0.003764).
Related
Questions
- Is oak harder than poplar?
- Yes. Northern red oak (red oak group) at 1,290 lbf1 and white oak (white oak group) at 1,360 lbf2 are harder than yellow-poplar at 540 lbf2.
- Which moves more, oak or poplar?
- Northern red oak (red oak group) and white oak (white oak group) move more than yellow-poplar across a flat-sawn board (CT 0.003044 and CT 0.003764 vs CT 0.002894).
References
- 1. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-10
- 2. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-11
- 3. Calculated from the two 12% Janka values: the difference divided by the lower value.
- 4. USDA Wood Handbook (FPL-GTR-282), Table 13-5, p. 13-17
- 5. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-5
- 6. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-6
- 7. USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8
- 8. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8).