Maple vs Oak wood

Sugar maple (hard maple) is harder, stronger in bending and stiffer than northern red oak (red oak group) and white oak (white oak group): 1,4501 vs 1,2901 and 1,3602 lbf, 7% to 12% harder3. Red maple (soft maple) is softer, weaker in bending and less stiff than both: 9501 vs 1,2901 and 1,3602 lbf. Movement across a flat-sawn board is split, from least to most: red maple CT 0.002894, northern red oak CT 0.003044, sugar maple CT 0.003534, and white oak CT 0.003764. Specific gravity (12% MC volume basis) is split: white oak 0.682, sugar maple 0.631, northern red oak 0.631, and red maple 0.541.

Side by side

PropertySugar maple (hard maple)Red maple (soft maple)Northern red oak (red oak group)White oak (white oak group)
Janka hardness, 12% MC1,450 lbf1; 6,400 N5950 lbf1; 4,200 N51,290 lbf1; 5,700 N51,360 lbf2; 6,000 N6
Janka hardness, green970 lbf1700 lbf11,000 lbf11,060 lbf2
Specific gravity, 12% MC volume basis0.6310.5410.6310.682
Bending strength (MOR), 12% MC15,800 psi1; 109,000 kPa513,400 psi1; 92,000 kPa514,300 psi1; 99,000 kPa515,200 psi2; 105,000 kPa6
Stiffness (MOE), 12% MC1.83 × 106 psi1; 12,600 MPa51.64 × 106 psi1; 11,300 MPa51.82 × 106 psi1; 12,500 MPa51.78 × 106 psi2; 12,300 MPa6
Shrinkage, green to oven-dryradial 4.8%, tangential 9.9%, volumetric 14.7%7radial 4%, tangential 8.2%, volumetric 12.6%7radial 4%, tangential 8.6%, volumetric 13.7%7radial 5.6%, tangential 10.5%, volumetric 16.3%7
T/R ratio (tangential ÷ radial)2.06, calculated82.05, calculated82.15, calculated81.88, calculated8
Movement coefficientsCR 0.00165; CT 0.003534CR 0.00137; CT 0.002894CR 0.00137; CT 0.003044CR 0.00194; CT 0.003764

Which to use

For a tabletop that must resist dents, sugar maple (hard maple) is the harder wood at 1,450 lbf1, against red maple (soft maple) at 950 lbf1.

For a wide flat-sawn panel, red maple moves less (CT 0.002894, against white oak (white oak group) at 0.003764).

Related

Questions

Is maple harder than oak?
It depends on the row. Sugar maple (hard maple) at 1,450 lbf1 and red maple (soft maple) at 950 lbf1; northern red oak (red oak group) at 1,290 lbf1 and white oak (white oak group) at 1,360 lbf2.
Which moves more, maple or oak?
It depends on the row. Sugar maple (hard maple) and red maple (soft maple) CT 0.003534 and CT 0.002894; northern red oak (red oak group) and white oak (white oak group) CT 0.003044 and CT 0.003764.

References

  • 1. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-10
  • 2. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-11
  • 3. Calculated from the two 12% Janka values: the difference divided by the lower value.
  • 4. USDA Wood Handbook (FPL-GTR-282), Table 13-5, p. 13-17
  • 5. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-5
  • 6. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-6
  • 7. USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8
  • 8. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8).