Red Oak vs White Oak wood
White oak is harder and stronger in bending than northern red oak but less stiff: 1,3601 vs 1,2902 lbf, 5% harder3; 15,2001 vs 14,3002 psi; 1.781 vs 1.822 × 106 psi. Northern red oak moves less across a flat-sawn board (CT 0.003044 vs 0.003764). White oak is denser (specific gravity 0.681 vs 0.632, 12% MC volume basis).
Side by side
| Property | Red oak (northern red oak) | White oak |
|---|---|---|
| Janka hardness, 12% MC | 1,290 lbf2; 5,700 N5 | 1,360 lbf1; 6,000 N6 |
| Janka hardness, green | 1,000 lbf2 | 1,060 lbf1 |
| Specific gravity, 12% MC volume basis | 0.632 | 0.681 |
| Bending strength (MOR), 12% MC | 14,300 psi2; 99,000 kPa5 | 15,200 psi1; 105,000 kPa6 |
| Stiffness (MOE), 12% MC | 1.82 × 106 psi2; 12,500 MPa5 | 1.78 × 106 psi1; 12,300 MPa6 |
| Shrinkage, green to oven-dry | radial 4%, tangential 8.6%, volumetric 13.7%7 | radial 5.6%, tangential 10.5%, volumetric 16.3%7 |
| T/R ratio (tangential ÷ radial) | 2.15, calculated8 | 1.88, calculated8 |
| Movement coefficients | CR 0.00137; CT 0.003044 | CR 0.00194; CT 0.003764 |
Which to use
For a tabletop that must resist dents, white oak is the harder wood at 1,360 lbf1, against northern red oak at 1,290 lbf2.
For a wide flat-sawn panel, northern red oak moves less (CT 0.003044, against white oak at 0.003764).
Related
Questions
- Is red oak harder than white oak?
- No. White oak at 1,360 lbf1 is harder than northern red oak at 1,290 lbf2.
- Which moves more, red oak or white oak?
- White oak moves more than northern red oak across a flat-sawn board (CT 0.003764 vs CT 0.003044).
References
- 1. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-11
- 2. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-10
- 3. Calculated from the two 12% Janka values: the difference divided by the lower value.
- 4. USDA Wood Handbook (FPL-GTR-282), Table 13-5, p. 13-17
- 5. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-5
- 6. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-6
- 7. USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8
- 8. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8).