Chinese JoineryChinese Joinery
Wood

Black walnut wood

Black walnut is a medium-hard hardwood2: 1,010 lbf1 on the Janka side-hardness test at 12% moisture, almost the same as teak (1,000 lbf3) and below northern red oak (1,290 lbf4).

It is moderately stiff5, and it moves about 0.27%6 across the width of a flat-sawn board for each 1% change in moisture content.

Key numbers

PropertyBlack walnut
Janka hardness, 12% MC1,010 lbf1; 4,500 N7
Janka hardness, green900 lbf1
Specific gravity, 12% MC volume basis0.551
Bending strength (MOR), 12% MC14,600 psi1; 101,000 kPa7
Stiffness (MOE), 12% MC1.68 × 106 psi1; 11,600 MPa7
Shrinkage, green to oven-dryradial 5.5%, tangential 7.8%, volumetric 12.8%8
T/R ratio (tangential ÷ radial)1.42, calculated9
Movement coefficientsCR 0.0019; CT 0.002746

How hard is black walnut?

01,0002,0003,0004,000black walnut 1,010 lbf

Ticks are the anchor woods, from eastern white pine to ipe; the scale is in lbf. See black walnut on the Janka chart.

How much does it move?

A 10-inch flat-sawn black walnut board going from 6% to 10% moisture content, the range the Handbook recommends for individual pieces of interior woodwork in most of the United States11, widens by 0.110 in10. A quartersawn board widens by 0.076 in10.

The coefficients apply from 6% to 14% moisture content12.

Try your own board in the wood movement calculator.

What it's used for

The heartwood varies from light to dark brown and the sapwood is nearly white. The wood is normally straight grained, easily worked with tools, and stable in use, and it suits natural finishes. It is valued for furniture, architectural woodwork, and decorative panels, and also for gunstocks, cabinets, and interior woodwork.13

Compare with

Questions

Is black walnut a hardwood?
Yes. Black walnut is a hardwood14. In the Handbook, hardwood means a broad-leaved angiosperm, not a wood that is necessarily hard. Specific gravity on a 12% MC volume basis is 0.551.
Is black walnut harder than teak?
Black walnut is harder than teak: 1,010 lbf1 versus 1,000 lbf3, both at 12% moisture.
How much does black walnut shrink?
From green to oven-dry, tangential shrinkage is 7.8% and radial shrinkage is 5.5%8. The T/R ratio is 1.42, calculated9.

References

  • 1. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-11
  • 2. Calculated from the 12% moisture Janka side-hardness values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 3. USDA Wood Handbook (FPL-GTR-282), Table 5-5b, p. 5-25
  • 4. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-10
  • 5. Calculated from the 12% moisture modulus of elasticity values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 6. USDA Wood Handbook (FPL-GTR-282), Table 13-5, p. 13-17
  • 7. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-6
  • 8. USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8
  • 9. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8).
  • 10. Calculated with Wood Handbook Eq. 13-3 (p. 13-16): 10 in × the coefficient × 4 percentage points. Tangential coefficient 0.00274; radial coefficient 0.0019.
  • 11. USDA Wood Handbook (FPL-GTR-282), Table 13-2, p. 13-5
  • 12. USDA Wood Handbook (FPL-GTR-282), ch. 13, p. 13-16
  • 13. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-10
  • 14. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-2