Poplar (yellow-poplar) wood
Poplar (yellow-poplar, Liriodendron tulipifera) is a soft hardwood2: 540 lbf1 on the Janka side-hardness test at 12% moisture, above eastern white pine (380 lbf3) and well below black cherry (950 lbf4).
It is flexible5, and it moves about 0.29%6 across the width of a flat-sawn board for each 1% change in moisture content.
Key numbers
| Property | Yellow-poplar |
|---|---|
| Janka hardness, 12% MC | 540 lbf1; 2,400 N7 |
| Janka hardness, green | 440 lbf1 |
| Specific gravity, 12% MC volume basis | 0.421 |
| Bending strength (MOR), 12% MC | 10,100 psi1; 70,000 kPa7 |
| Stiffness (MOE), 12% MC | 1.58 × 106 psi1; 10,900 MPa7 |
| Shrinkage, green to oven-dry | radial 4.6%, tangential 8.2%, volumetric 12.7%8 |
| T/R ratio (tangential ÷ radial) | 1.78, calculated9 |
| Movement coefficients | CR 0.00158; CT 0.002896 |
How hard is poplar (yellow-poplar)?
Ticks are the anchor woods, from eastern white pine to ipe; the scale is in lbf. See yellow-poplar on the Janka chart.
How much does it move?
A 10-inch flat-sawn yellow-poplar board going from 6% to 10% moisture content, the range the Handbook recommends for individual pieces of interior woodwork in most of the United States11, widens by 0.116 in10. A quartersawn board widens by 0.063 in10.
The coefficients apply from 6% to 14% moisture content12.
Try your own board in the wood movement calculator.
What it's used for
The sapwood is white and the heartwood is yellowish brown, sometimes streaked with purple, green, black, blue, or red. The wood is generally straight grained and comparatively uniform in texture, and it is stable after drying. Lumber is used for furniture, interior molding, siding, cabinets, and musical instruments, and the wood is also made into plywood for paneling and furniture.13
Compare with
Questions
- Is poplar a hardwood?
- Yes. Poplar is a hardwood14. In the Handbook, hardwood means a broad-leaved angiosperm, not a wood that is necessarily hard. Specific gravity on a 12% MC volume basis is 0.421.
- Is poplar harder than eastern white pine?
- Poplar is harder than eastern white pine: 540 lbf1 versus 380 lbf3, both at 12% moisture.
- How much does poplar shrink?
- From green to oven-dry, tangential shrinkage is 8.2% and radial shrinkage is 4.6%8. The T/R ratio is 1.78, calculated9.
References
- 1. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-11
- 2. Calculated from the 12% moisture Janka side-hardness values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
- 3. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-12
- 4. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-9
- 5. Calculated from the 12% moisture modulus of elasticity values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
- 6. USDA Wood Handbook (FPL-GTR-282), Table 13-5, p. 13-17
- 7. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-6
- 8. USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8
- 9. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8).
- 10. Calculated with Wood Handbook Eq. 13-3 (p. 13-16): 10 in × the coefficient × 4 percentage points. Tangential coefficient 0.00289; radial coefficient 0.00158.
- 11. USDA Wood Handbook (FPL-GTR-282), Table 13-2, p. 13-5
- 12. USDA Wood Handbook (FPL-GTR-282), ch. 13, p. 13-16
- 13. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-11
- 14. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-2