Chinese JoineryChinese Joinery
Wood

Southern yellow pine (longleaf pine) wood

Southern yellow pine (longleaf pine, Pinus palustris) is a medium-soft softwood2: 870 lbf1 on the Janka side-hardness test at 12% moisture, below black cherry (950 lbf4) and well above yellow-poplar (540 lbf3).

It is moderately stiff5, and it moves about 0.25%6 across the width of a flat-sawn board for each 1% change in moisture content.

Key numbers

PropertyLongleaf pine
Janka hardness, 12% MC870 lbf1; 3,900 N7
Janka hardness, green590 lbf1
Specific gravity, 12% MC volume basis0.591
Bending strength (MOR), 12% MC14,500 psi1; 100,000 kPa7
Stiffness (MOE), 12% MC1.98 × 106 psi1; 13,700 MPa7
Shrinkage, green to oven-dryradial 5.1%, tangential 7.5%, volumetric 12.2%8
T/R ratio (tangential ÷ radial)1.47, calculated9
Movement coefficientsCR 0.00137; CT 0.002486

How hard is southern yellow pine (longleaf pine)?

01,0002,0003,0004,000longleaf pine 870 lbf

Ticks are the anchor woods, from eastern white pine to ipe; the scale is in lbf. See longleaf pine on the Janka chart.

How much does it move?

A 10-inch flat-sawn longleaf pine board going from 6% to 10% moisture content, the range the Handbook recommends for individual pieces of interior woodwork in most of the United States11, widens by 0.099 in10. A quartersawn board widens by 0.055 in10.

The coefficients apply from 6% to 14% moisture content12.

Try your own board in the wood movement calculator.

What it's used for

The southern pines look quite similar: the sapwood is yellowish white and the heartwood is reddish brown. Denser southern pine is used for heavy construction, and the lumber is also used for interior woodwork, boxes, pallets, crates, cooperage, and structural plywood.13

Compare with

Questions

Is southern yellow pine a hardwood?
No. Southern yellow pine is a softwood14. Softwoods are conifers. The name is botanical, not a hardness ranking. Specific gravity on a 12% MC volume basis is 0.591.
Is southern yellow pine harder than black cherry?
Southern yellow pine is softer than black cherry: 870 lbf1 versus 950 lbf4, both at 12% moisture.
How much does southern yellow pine shrink?
From green to oven-dry, tangential shrinkage is 7.5% and radial shrinkage is 5.1%8. The T/R ratio is 1.47, calculated9.

References

  • 1. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-12
  • 2. Calculated from the 12% moisture Janka side-hardness values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 3. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-11
  • 4. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-9
  • 5. Calculated from the 12% moisture modulus of elasticity values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 6. USDA Wood Handbook (FPL-GTR-282), Table 13-5, p. 13-17
  • 7. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-7
  • 8. USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8
  • 9. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8).
  • 10. Calculated with Wood Handbook Eq. 13-3 (p. 13-16): 10 in × the coefficient × 4 percentage points. Tangential coefficient 0.00248; radial coefficient 0.00137.
  • 11. USDA Wood Handbook (FPL-GTR-282), Table 13-2, p. 13-5
  • 12. USDA Wood Handbook (FPL-GTR-282), ch. 13, p. 13-16
  • 13. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-15
  • 14. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-2