Soft maple (red maple, Acer rubrum) is a medium-hard hardwood2: 950 lbf1 on the Janka side-hardness test at 12% moisture, almost the same as teak (1,000 lbf4) and well above yellow-poplar (540 lbf3).

It is flexible5, and it moves about 0.29%6 across the width of a flat-sawn board for each 1% change in moisture content.

Key numbers

PropertyRed maple
Janka hardness, 12% MC950 lbf1; 4,200 N7
Janka hardness, green700 lbf1
Specific gravity, 12% MC volume basis0.541
Bending strength (MOR), 12% MC13,400 psi1; 92,000 kPa7
Stiffness (MOE), 12% MC1.64 × 106 psi1; 11,300 MPa7
Shrinkage, green to oven-dryradial 4%, tangential 8.2%, volumetric 12.6%8
T/R ratio (tangential ÷ radial)2.05, calculated9
Movement coefficientsCR 0.00137; CT 0.002896

How hard is soft maple (red maple)?

01,0002,0003,0004,000red maple 950 lbf

Ticks are the anchor woods, from eastern white pine to ipe; the scale is in lbf. See red maple on the Janka chart.

How much does it move?

A 10-inch flat-sawn red maple board going from 6% to 10% moisture content, the range the Handbook recommends for individual pieces of interior woodwork in most of the United States11, widens by 0.116 in10. A quartersawn board widens by 0.055 in10.

The coefficients apply from 6% to 14% moisture content12.

Try your own board in the wood movement calculator.

What it's used for

Heartwood and sapwood look much like hard maple, and the sapwood is somewhat lighter in color than the heartwood. The wood of red maple resembles hard maple. Soft maple is used for railroad ties, boxes, pallets, crates, furniture, veneer, woodenware, and novelties.13

Compare with

Questions

Is soft maple a hardwood?
Yes. Soft maple is a hardwood14. In the Handbook, hardwood means a broad-leaved angiosperm, not a wood that is necessarily hard. Specific gravity on a 12% MC volume basis is 0.541.
Is soft maple harder than black cherry?
Soft maple is the same hardness as black cherry: 950 lbf1 versus 950 lbf15, both at 12% moisture.
How much does soft maple shrink?
From green to oven-dry, tangential shrinkage is 8.2% and radial shrinkage is 4%8. The T/R ratio is 2.05, calculated9.

References

  • 1. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-10
  • 2. Calculated from the 12% moisture Janka side-hardness values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 3. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-11
  • 4. USDA Wood Handbook (FPL-GTR-282), Table 5-5b, p. 5-25
  • 5. Calculated from the 12% moisture modulus of elasticity values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 6. USDA Wood Handbook (FPL-GTR-282), Table 13-5, p. 13-17
  • 7. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-5
  • 8. USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8
  • 9. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8).
  • 10. Calculated with Wood Handbook Eq. 13-3 (p. 13-16): 10 in × the coefficient × 4 percentage points. Tangential coefficient 0.00289; radial coefficient 0.00137.
  • 11. USDA Wood Handbook (FPL-GTR-282), Table 13-2, p. 13-5
  • 12. USDA Wood Handbook (FPL-GTR-282), ch. 13, p. 13-16
  • 13. USDA Wood Handbook (FPL-GTR-282), ch. 2, pp. 2-8–2-9
  • 14. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-2
  • 15. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-9