Chinese JoineryChinese Joinery
Wood

Birch (yellow birch) wood

Birch (yellow birch, Betula alleghaniensis) is a medium-hard hardwood2: 1,260 lbf1 on the Janka side-hardness test at 12% moisture, almost the same as northern red oak (1,290 lbf4) and above black walnut (1,010 lbf3).

It is stiff5, and it moves about 0.34%6 across the width of a flat-sawn board for each 1% change in moisture content.

Key numbers

PropertyYellow birch
Janka hardness, 12% MC1,260 lbf1; 5,600 N7
Janka hardness, green780 lbf1
Specific gravity, 12% MC volume basis0.621
Bending strength (MOR), 12% MC16,600 psi1; 114,000 kPa7
Stiffness (MOE), 12% MC2.01 × 106 psi1; 13,900 MPa7
Shrinkage, green to oven-dryradial 7.3%, tangential 9.5%, volumetric 16.8%8
T/R ratio (tangential ÷ radial)1.30, calculated9
Movement coefficientsCR 0.00256; CT 0.003386

How hard is birch (yellow birch)?

01,0002,0003,0004,000yellow birch 1,260 lbf

Ticks are the anchor woods, from eastern white pine to ipe; the scale is in lbf. See yellow birch on the Janka chart.

How much does it move?

A 10-inch flat-sawn yellow birch board going from 6% to 10% moisture content, the range the Handbook recommends for individual pieces of interior woodwork in most of the United States11, widens by 0.135 in10. A quartersawn board widens by 0.102 in10.

The coefficients apply from 6% to 14% moisture content12.

Try your own board in the wood movement calculator.

What it's used for

Yellow birch has white sapwood and light reddish-brown heartwood, and the wood is fine and uniform in texture. Yellow and sweet birch lumber is used for furniture, boxes, baskets, crates, woodenware, cooperage, interior woodwork, and doors. Veneer plywood is used for doors, furniture, paneling, cabinets, and other specialty uses.13

Compare with

Questions

Is birch a hardwood?
Yes. Birch is a hardwood14. In the Handbook, hardwood means a broad-leaved angiosperm, not a wood that is necessarily hard. Specific gravity on a 12% MC volume basis is 0.621.
Is birch harder than northern red oak?
Birch is softer than northern red oak: 1,260 lbf1 versus 1,290 lbf4, both at 12% moisture.
How much does birch shrink?
From green to oven-dry, tangential shrinkage is 9.5% and radial shrinkage is 7.3%8. The T/R ratio is 1.30, calculated9.

References

  • 1. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-9
  • 2. Calculated from the 12% moisture Janka side-hardness values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 3. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-11
  • 4. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-10
  • 5. Calculated from the 12% moisture modulus of elasticity values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 6. USDA Wood Handbook (FPL-GTR-282), Table 13-5, p. 13-17
  • 7. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-4
  • 8. USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8
  • 9. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8).
  • 10. Calculated with Wood Handbook Eq. 13-3 (p. 13-16): 10 in × the coefficient × 4 percentage points. Tangential coefficient 0.00338; radial coefficient 0.00256.
  • 11. USDA Wood Handbook (FPL-GTR-282), Table 13-2, p. 13-5
  • 12. USDA Wood Handbook (FPL-GTR-282), ch. 13, p. 13-16
  • 13. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-5
  • 14. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-2