Maple vs Poplar wood
Sugar maple (hard maple) is harder, stronger in bending and stiffer than yellow-poplar: 1,4501 vs 5402 lbf, 169% harder3. Red maple (soft maple) is harder, stronger in bending and stiffer than yellow-poplar: 9501 vs 5402 lbf, 76% harder3. Movement across a flat-sawn board is split, from least to most: red maple CT 0.002894, yellow-poplar CT 0.002894, and sugar maple CT 0.003534. Sugar maple and red maple are denser (specific gravity 0.631 and 0.541 vs 0.422, 12% MC volume basis).
Side by side
| Property | Sugar maple (hard maple) | Red maple (soft maple) | Poplar (yellow-poplar) |
|---|---|---|---|
| Janka hardness, 12% MC | 1,450 lbf1; 6,400 N5 | 950 lbf1; 4,200 N5 | 540 lbf2; 2,400 N6 |
| Janka hardness, green | 970 lbf1 | 700 lbf1 | 440 lbf2 |
| Specific gravity, 12% MC volume basis | 0.631 | 0.541 | 0.422 |
| Bending strength (MOR), 12% MC | 15,800 psi1; 109,000 kPa5 | 13,400 psi1; 92,000 kPa5 | 10,100 psi2; 70,000 kPa6 |
| Stiffness (MOE), 12% MC | 1.83 × 106 psi1; 12,600 MPa5 | 1.64 × 106 psi1; 11,300 MPa5 | 1.58 × 106 psi2; 10,900 MPa6 |
| Shrinkage, green to oven-dry | radial 4.8%, tangential 9.9%, volumetric 14.7%7 | radial 4%, tangential 8.2%, volumetric 12.6%7 | radial 4.6%, tangential 8.2%, volumetric 12.7%7 |
| T/R ratio (tangential ÷ radial) | 2.06, calculated8 | 2.05, calculated8 | 1.78, calculated8 |
| Movement coefficients | CR 0.00165; CT 0.003534 | CR 0.00137; CT 0.002894 | CR 0.00158; CT 0.002894 |
Which to use
For a tabletop that must resist dents, sugar maple (hard maple) is the harder wood at 1,450 lbf1, against yellow-poplar at 540 lbf2.
For a wide flat-sawn panel, red maple (soft maple) moves less (CT 0.002894, against sugar maple at 0.003534).
Related
Questions
- Is maple harder than poplar?
- Yes. Sugar maple (hard maple) at 1,450 lbf1 and red maple (soft maple) at 950 lbf1 are harder than yellow-poplar at 540 lbf2.
- Which moves more, maple or poplar?
- It depends on the row. Sugar maple (hard maple) and red maple (soft maple) CT 0.003534 and CT 0.002894; yellow-poplar CT 0.002894.
References
- 1. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-10
- 2. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-11
- 3. Calculated from the two 12% Janka values: the difference divided by the lower value.
- 4. USDA Wood Handbook (FPL-GTR-282), Table 13-5, p. 13-17
- 5. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-5
- 6. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-6
- 7. USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8
- 8. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8).