Chinese JoineryChinese Joinery
Wood

Teak vs Walnut wood

Black walnut is harder and stiffer than teak, with the same bending strength: 1,0101 vs 1,0002 lbf, 1% harder3; 14,60012 psi each; 1.681 vs 1.552 × 106 psi. Teak moves less across a flat-sawn board (CT 0.002014 vs 0.002745). Teak is denser (specific gravity 0.552 vs 0.511, green volume basis).

Side by side

PropertyTeakBlack walnut
Janka hardness, 12% MC1,000 lbf2; 4,400 N61,010 lbf1; 4,500 N7
Janka hardness, green930 lbf2900 lbf1
Specific gravity, green volume basis0.5520.511
Bending strength (MOR), 12% MC14,600 psi2; 100,700 kPa614,600 psi1; 101,000 kPa7
Stiffness (MOE), 12% MC1.55 × 106 psi2; 10,700 MPa61.68 × 106 psi1; 11,600 MPa7
Shrinkage, green to oven-dryradial 2.5%, tangential 5.8%, volumetric 7%8radial 5.5%, tangential 7.8%, volumetric 12.8%9
T/R ratio (tangential ÷ radial)2.32, calculated101.42, calculated11
Movement coefficientsCR 0.00085, calculated; CT 0.00201, calculated4CR 0.0019; CT 0.002745

Which to use

For a tabletop that must resist dents, black walnut is the harder wood at 1,010 lbf1, against teak at 1,000 lbf2.

For a wide flat-sawn panel, teak moves less (CT 0.002014, against black walnut at 0.002745).

Related

Questions

Is teak harder than walnut?
No. Black walnut at 1,010 lbf1 is harder than teak at 1,000 lbf2.
Which moves more, teak or walnut?
Black walnut moves more than teak across a flat-sawn board (CT 0.002745 vs CT 0.002014).

References

  • 1. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-11
  • 2. USDA Wood Handbook (FPL-GTR-282), Table 5-5b, p. 5-25
  • 3. Calculated from the two 12% Janka values: the difference divided by the lower value.
  • 4. Calculated with Wood Handbook Eq. 13-2 (p. 13-16) from Table 4-4 (p. 4-9)
  • 5. USDA Wood Handbook (FPL-GTR-282), Table 13-5, p. 13-17
  • 6. USDA Wood Handbook (FPL-GTR-282), Table 5-5a, p. 5-21
  • 7. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-6
  • 8. USDA Wood Handbook (FPL-GTR-282), Table 4-4, p. 4-9
  • 9. USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8
  • 10. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-4, p. 4-9).
  • 11. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8).