Ipe is a very hard hardwood2: 3,680 lbf1 on the Janka side-hardness test at 12% moisture, well above shagbark hickory (1,880 lbf3).

It is stiff4, and it moves about 0.28%5 across the width of a flat-sawn board for each 1% change in moisture content.

Key numbers

PropertyIpe
Janka hardness, 12% MC3,680 lbf1; 16,400 N6
Janka hardness, green3,060 lbf1
Specific gravity, green volume basis0.921
Bending strength (MOR), 12% MC25,400 psi1; 175,100 kPa6
Stiffness (MOE), 12% MC3.14 × 106 psi1; 21,600 MPa6
Shrinkage, green to oven-dryradial 6.6%, tangential 8%, volumetric 13.2%7
T/R ratio (tangential ÷ radial)1.21, calculated8
Movement coefficientsCR 0.0023, calculated; CT 0.00282, calculated5

How hard is ipe?

01,0002,0003,0004,000ipe 3,680 lbf

Ticks are the anchor woods, from eastern white pine to ipe; the scale is in lbf. See ipe on the Janka chart.

How much does it move?

A 10-inch flat-sawn ipe board going from 6% to 10% moisture content, the range the Handbook recommends for individual pieces of interior woodwork in most of the United States10, widens by 0.113 in9. A quartersawn board widens by 0.092 in9.

The coefficients apply from 6% to 14% moisture content11.

Try your own board in the wood movement calculator.

What it's used for

The sapwood is yellowish gray or gray-brown and the heartwood is light to dark olive brown, with a fine to medium texture and grain that is straight to very irregular and often narrowly interlocked. The wood is moderately difficult to machine, but glassy smooth surfaces can be produced. It is used for heavy-duty construction, flooring, decks, ties, turnery, tool handles, and decorative veneers.12

Compare with

Questions

Is ipe a hardwood?
Yes. Ipe is a hardwood13. In the Handbook, hardwood means a broad-leaved angiosperm, not a wood that is necessarily hard. Specific gravity on a green volume basis is 0.921.
Is ipe harder than shagbark hickory?
Ipe is harder than shagbark hickory: 3,680 lbf1 versus 1,880 lbf3, both at 12% moisture.
How much does ipe shrink?
From green to oven-dry, tangential shrinkage is 8% and radial shrinkage is 6.6%7. The T/R ratio is 1.21, calculated8.

References

  • 1. USDA Wood Handbook (FPL-GTR-282), Table 5-5b, p. 5-23
  • 2. Calculated from the 12% moisture Janka side-hardness values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 3. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-10
  • 4. Calculated from the 12% moisture modulus of elasticity values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 5. Calculated with Wood Handbook Eq. 13-2 (p. 13-16) from Table 4-4 (p. 4-9)
  • 6. USDA Wood Handbook (FPL-GTR-282), Table 5-5a, p. 5-19
  • 7. USDA Wood Handbook (FPL-GTR-282), Table 4-4, p. 4-9
  • 8. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-4, p. 4-9).
  • 9. Calculated with Wood Handbook Eq. 13-3 (p. 13-16): 10 in × the coefficient × 4 percentage points. Tangential coefficient 0.00282; radial coefficient 0.0023.
  • 10. USDA Wood Handbook (FPL-GTR-282), Table 13-2, p. 13-5
  • 11. USDA Wood Handbook (FPL-GTR-282), ch. 13, p. 13-16
  • 12. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-25
  • 13. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-2