Ipe is harder, stronger in bending and stiffer than teak: 3,6801 vs 1,0002 lbf, 268% harder3; 25,4001 vs 14,6002 psi; 3.141 vs 1.552 × 106 psi. Teak moves less across a flat-sawn board (CT 0.002014 vs 0.002824). Ipe is denser (specific gravity 0.921 vs 0.552, green volume basis).

Side by side

PropertyIpeTeak
Janka hardness, 12% MC3,680 lbf1; 16,400 N51,000 lbf2; 4,400 N6
Janka hardness, green3,060 lbf1930 lbf2
Specific gravity, green volume basis0.9210.552
Bending strength (MOR), 12% MC25,400 psi1; 175,100 kPa514,600 psi2; 100,700 kPa6
Stiffness (MOE), 12% MC3.14 × 106 psi1; 21,600 MPa51.55 × 106 psi2; 10,700 MPa6
Shrinkage, green to oven-dryradial 6.6%, tangential 8%, volumetric 13.2%7radial 2.5%, tangential 5.8%, volumetric 7%7
T/R ratio (tangential ÷ radial)1.21, calculated82.32, calculated8
Movement coefficientsCR 0.0023, calculated; CT 0.00282, calculated4CR 0.00085, calculated; CT 0.00201, calculated4

Which to use

For a tabletop that must resist dents, ipe is the harder wood at 3,680 lbf1, against teak at 1,000 lbf2.

For a wide flat-sawn panel, teak moves less (CT 0.002014, against ipe at 0.002824).

Related

Questions

Is ipe harder than teak?
Yes. Ipe at 3,680 lbf1 is harder than teak at 1,000 lbf2.
Which moves more, ipe or teak?
Ipe moves more than teak across a flat-sawn board (CT 0.002824 vs CT 0.002014).

References

  • 1. USDA Wood Handbook (FPL-GTR-282), Table 5-5b, p. 5-23
  • 2. USDA Wood Handbook (FPL-GTR-282), Table 5-5b, p. 5-25
  • 3. Calculated from the two 12% Janka values: the difference divided by the lower value.
  • 4. Calculated with Wood Handbook Eq. 13-2 (p. 13-16) from Table 4-4 (p. 4-9)
  • 5. USDA Wood Handbook (FPL-GTR-282), Table 5-5a, p. 5-19
  • 6. USDA Wood Handbook (FPL-GTR-282), Table 5-5a, p. 5-21
  • 7. USDA Wood Handbook (FPL-GTR-282), Table 4-4, p. 4-9
  • 8. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-4, p. 4-9).