Lignum vitae is the hardest of the 169 woods rated in the USDA Wood Handbook at 4,500 lbf1, and ceiba the softest at 240 lbf23. Of the three woods the table opens with, sugar maple is the hardest at 1,450 lbf4, 44% harder than black walnut at 1,010 lbf56, with white oak at 1,360 lbf5 between them.

    Choose two to four woods. The table starts with black walnut, white oak, and sugar maple.

    PropertyBlack walnutWhite oakSugar maple
    Janka hardness, 12% MC1,010 lbf5; 4,500 N71,360 lbf5; 6,000 N71,450 lbf4; 6,400 N8
    Janka hardness, green900 lbf51,060 lbf5970 lbf4
    Specific gravity, 12% MC volume basis0.5550.6850.634
    Bending strength (MOR), 12% MC14,600 psi5; 101,000 kPa715,200 psi5; 105,000 kPa715,800 psi4; 109,000 kPa8
    Stiffness (MOE), 12% MC1.68 × 106 psi5; 11,600 MPa71.78 × 106 psi5; 12,300 MPa71.83 × 106 psi4; 12,600 MPa8
    Shrinkage, green to oven-dryradial 5.5%, tangential 7.8%, volumetric 12.8%9radial 5.6%, tangential 10.5%, volumetric 16.3%9radial 4.8%, tangential 9.9%, volumetric 14.7%9
    T/R ratio (tangential ÷ radial)1.42, calculated101.88, calculated102.06, calculated10
    Movement coefficientsCR 0.0019; CT 0.0027411CR 0.00194; CT 0.0037611CR 0.00165; CT 0.0035311

    All woods · Janka hardness chart

    References

    • 1. USDA Wood Handbook (FPL-GTR-282), Table 5-5b, p. 5-23
    • 2. USDA Wood Handbook (FPL-GTR-282), Table 5-5b, p. 5-22
    • 3. Calculated from the 12% moisture Janka side-hardness values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
    • 4. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-10
    • 5. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-11
    • 6. Calculated from the two 12% Janka values: the difference divided by the lower value.
    • 7. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-6
    • 8. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-5
    • 9. USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8
    • 10. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8).
    • 11. USDA Wood Handbook (FPL-GTR-282), Table 13-5, p. 13-17