Hickory vs Walnut wood
Shagbark hickory is harder, stronger in bending and stiffer than black walnut: 1,8801 vs 1,0102 lbf, 86% harder3. Pecan is harder and stiffer than black walnut but weaker in bending: 1,8201 vs 1,0102 lbf, 80% harder3. Black walnut moves less across a flat-sawn board (CT 0.002744 vs 0.00411 (Handbook group row “Hickory, true”)5 and 0.00315 (Handbook group row “Hickory, pecan”)6). Shagbark hickory and pecan are denser (specific gravity 0.721 and 0.661 vs 0.552, 12% MC volume basis).
Side by side
| Property | Shagbark hickory | Pecan | Black walnut |
|---|---|---|---|
| Janka hardness, 12% MC | 1,880 lbf1; 8,400 N7 | 1,820 lbf1; 8,100 N7 | 1,010 lbf2; 4,500 N8 |
| Janka hardness, green | 1,460 lbf1 | 1,310 lbf1 | 900 lbf2 |
| Specific gravity, 12% MC volume basis | 0.721 | 0.661 | 0.552 |
| Bending strength (MOR), 12% MC | 20,200 psi1; 139,000 kPa7 | 13,700 psi1; 94,000 kPa7 | 14,600 psi2; 101,000 kPa8 |
| Stiffness (MOE), 12% MC | 2.16 × 106 psi1; 14,900 MPa7 | 1.73 × 106 psi1; 11,900 MPa7 | 1.68 × 106 psi2; 11,600 MPa8 |
| Shrinkage, green to oven-dry | radial 7%, tangential 10.5%, volumetric 16.7%9 | radial 4.9%, tangential 8.9%, volumetric 13.6% (Handbook group row “Hickory, pecan”)10 | radial 5.5%, tangential 7.8%, volumetric 12.8%9 |
| T/R ratio (tangential ÷ radial) | 1.50, calculated11 | 1.82, calculated12 | 1.42, calculated11 |
| Movement coefficients | CR 0.00259; CT 0.00411 (Handbook group row “Hickory, true”)5 | CR 0.00169; CT 0.00315 (Handbook group row “Hickory, pecan”)6 | CR 0.0019; CT 0.002744 |
Movement coefficients for shagbark hickory are the Handbook’s group row “Hickory, true”, printed once for the whole group rather than measured separately for each species. Shrinkage and movement coefficients for pecan are the Handbook’s group row “Hickory, pecan”, printed once for the whole group rather than measured separately for each species.
Which to use
For a tabletop that must resist dents, shagbark hickory is the harder wood at 1,880 lbf1, against black walnut at 1,010 lbf2.
For a wide flat-sawn panel, black walnut moves less (CT 0.002744, against shagbark hickory at 0.00411 (Handbook group row “Hickory, true”)5).
Related
Questions
- Is hickory harder than walnut?
- Yes. Shagbark hickory at 1,880 lbf1 and pecan at 1,820 lbf1 are harder than black walnut at 1,010 lbf2.
- Which moves more, hickory or walnut?
- Shagbark hickory and pecan move more than black walnut across a flat-sawn board (CT 0.00411 (Handbook group row “Hickory, true”)5 and CT 0.00315 (Handbook group row “Hickory, pecan”)6 vs CT 0.002744).
References
- 1. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-10
- 2. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-11
- 3. Calculated from the two 12% Janka values: the difference divided by the lower value.
- 4. USDA Wood Handbook (FPL-GTR-282), Table 13-5, p. 13-17
- 5. USDA Wood Handbook (FPL-GTR-282), Table 13-5, p. 13-17 (row “Hickory, true”)
- 6. USDA Wood Handbook (FPL-GTR-282), Table 13-5, p. 13-17 (row “Hickory, pecan”)
- 7. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-5
- 8. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-6
- 9. USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8
- 10. USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8 (row “Hickory, pecan”)
- 11. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8).
- 12. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8 (row “Hickory, pecan”)).