Chinese JoineryChinese Joinery
Wood

Western hemlock wood

Western hemlock is a softwood, soft on the Janka scale2: 540 lbf1 on the Janka side-hardness test at 12% moisture, above eastern white pine (380 lbf1) and well below black cherry (950 lbf3).

It is flexible4, and it moves about 0.27%5 across the width of a flat-sawn board for each 1% change in moisture content.

Key numbers

PropertyWestern hemlock
Janka hardness, 12% MC540 lbf1; 2,400 N6
Janka hardness, green410 lbf1
Specific gravity, 12% MC volume basis0.451
Bending strength (MOR), 12% MC11,300 psi1; 78,000 kPa6
Stiffness (MOE), 12% MC1.63 × 106 psi1; 11,300 MPa6
Shrinkage, green to oven-dryradial 4.2%, tangential 7.8%, volumetric 12.4%7
T/R ratio (tangential ÷ radial)1.86, calculated8
Movement coefficientsCR 0.00144; CT 0.002745

How hard is western hemlock?

01,0002,0003,0004,000western hemlock 540 lbf

Ticks are the anchor woods, from eastern white pine to ipe; the scale is in lbf. See western hemlock on the Janka chart.

How much does it move?

A 10-inch flat-sawn western hemlock board going from 6% to 10% moisture content, the range the Handbook recommends for individual pieces of interior woodwork in most of the United States10, widens by 0.110 in9. A quartersawn board widens by 0.058 in9.

The coefficients apply from 6% to 14% moisture content11.

Try your own board in the wood movement calculator.

What it's used for

The heartwood and sapwood are almost white with a purplish tinge, and the sapwood is sometimes lighter. Small, sound, black knots are common and usually tight. Western hemlock is used for pulpwood, lumber, and plywood, and the lumber is used for sheathing, siding, joists, studs, flooring, furniture, and ladders.12

Compare with

Questions

Is western hemlock a hardwood?
No. Western hemlock is a softwood13. Softwoods are conifers. The name is botanical, not a hardness ranking. Specific gravity on a 12% MC volume basis is 0.451.
Is western hemlock harder than yellow-poplar?
Western hemlock is the same hardness as yellow-poplar: 540 lbf1 versus 540 lbf14, both at 12% moisture.
How much does western hemlock shrink?
From green to oven-dry, tangential shrinkage is 7.8% and radial shrinkage is 4.2%7. The T/R ratio is 1.86, calculated8.

References

  • 1. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-12
  • 2. Calculated from the 12% moisture Janka side-hardness values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 3. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-9
  • 4. Calculated from the 12% moisture modulus of elasticity values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 5. USDA Wood Handbook (FPL-GTR-282), Table 13-5, p. 13-17
  • 6. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-7
  • 7. USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8
  • 8. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8).
  • 9. Calculated with Wood Handbook Eq. 13-3 (p. 13-16): 10 in × the coefficient × 4 percentage points. Tangential coefficient 0.00274; radial coefficient 0.00144.
  • 10. USDA Wood Handbook (FPL-GTR-282), Table 13-2, p. 13-5
  • 11. USDA Wood Handbook (FPL-GTR-282), ch. 13, p. 13-16
  • 12. USDA Wood Handbook (FPL-GTR-282), ch. 2, pp. 2-12–2-13
  • 13. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-2
  • 14. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-11