Chinese JoineryChinese Joinery
Wood

Redwood wood

Redwood in the Handbook is two rows. Redwood (old-growth) is 480 lbf1; redwood (young-growth) is 420 lbf1. Redwood (old-growth) is a softwood, soft on the Janka scale2.

It is flexible3, and it moves about 0.21%4 across the width of a flat-sawn board for each 1% change in moisture content.

Redwood (young-growth) moves about 0.23% (Handbook row “Redwood, second-growth”)5 per 1% moisture change, flat-sawn.

Key numbers

PropertyRedwood (old-growth)Redwood (young-growth)
Janka hardness, 12% MC480 lbf1; 2,100 N6420 lbf1; 1,900 N6
Janka hardness, green410 lbf1350 lbf1
Specific gravity, 12% MC volume basis0.410.351
Bending strength (MOR), 12% MC10,000 psi1; 69,000 kPa67,900 psi1; 54,000 kPa6
Stiffness (MOE), 12% MC1.34 × 106 psi1; 9,200 MPa61.1 × 106 psi1; 7,600 MPa6
Shrinkage, green to oven-dryradial 2.6%, tangential 4.4%, volumetric 6.8%7radial 2.2%, tangential 4.9%, volumetric 7%7
T/R ratio (tangential ÷ radial)1.69, calculated82.23, calculated8
Movement coefficientsCR 0.0012; CT 0.002054CR 0.00101; CT 0.00229 (Handbook row “Redwood, second-growth”)5

Movement coefficients for redwood (young-growth) are printed in the Handbook under the row “Redwood, second-growth”.

How hard is redwood?

01,0002,0003,0004,000redwood (young-growth) 420 lbfredwood (old-growth) 480 lbf

Ticks are the anchor woods, from eastern white pine to ipe; the scale is in lbf. See redwood (old-growth) on the Janka chart and redwood (young-growth).

How much does it move?

A 10-inch flat-sawn redwood (old-growth) board going from 6% to 10% moisture content, the range the Handbook recommends for individual pieces of interior woodwork in most of the United States10, widens by 0.082 in9. A quartersawn board widens by 0.048 in9.

A 10-inch flat-sawn redwood (young-growth) board going from 6% to 10% moisture content, the range the Handbook recommends for individual pieces of interior woodwork in most of the United States10, widens by 0.092 in11. A quartersawn board widens by 0.040 in11. Both figures use the coefficients of the Handbook row “Redwood, second-growth”.

The coefficients apply from 6% to 14% moisture content12.

Try your own board in the wood movement calculator.

What it's used for

Redwood (old-growth). The heartwood varies from a light cherry red to dark mahogany, and the narrow sapwood is almost white. Old-growth wood is easy to work, generally straight grained, and shrinks and swells comparatively little, and old-growth heartwood has high decay resistance. Most redwood lumber is used for building, including siding, millwork, decking, tanks, and outdoor furniture.13

Redwood (young-growth). The heartwood varies from a light cherry red to dark mahogany, and the narrow sapwood is almost white. Heartwood from second-growth trees generally has low to moderate decay resistance. Most redwood lumber is used for building, including siding, millwork, decking, and outdoor furniture.13

Compare with

Questions

Is redwood a hardwood?
No. Redwood is a softwood14. Softwoods are conifers. The name is botanical, not a hardness ranking. Specific gravity on a 12% MC volume basis is 0.41.
Is redwood harder than yellow-poplar?
Redwood is softer than yellow-poplar: 480 lbf1 versus 540 lbf15, both at 12% moisture.
How much does redwood shrink?
From green to oven-dry, tangential shrinkage is 4.4% and radial shrinkage is 2.6%7. The T/R ratio is 1.69, calculated8.

References

  • 1. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-13
  • 2. Calculated from the 12% moisture Janka side-hardness values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 3. Calculated from the 12% moisture modulus of elasticity values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 4. USDA Wood Handbook (FPL-GTR-282), Table 13-5, p. 13-17
  • 5. USDA Wood Handbook (FPL-GTR-282), Table 13-5, p. 13-17 (row “Redwood, second-growth”)
  • 6. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-8
  • 7. USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8
  • 8. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8).
  • 9. Calculated with Wood Handbook Eq. 13-3 (p. 13-16): 10 in × the coefficient × 4 percentage points. Tangential coefficient 0.00205; radial coefficient 0.0012.
  • 10. USDA Wood Handbook (FPL-GTR-282), Table 13-2, p. 13-5
  • 11. Calculated with Wood Handbook Eq. 13-3 (p. 13-16): 10 in × the coefficient × 4 percentage points. Tangential coefficient 0.00229; radial coefficient 0.00101.
  • 12. USDA Wood Handbook (FPL-GTR-282), ch. 13, p. 13-16
  • 13. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-17
  • 14. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-2
  • 15. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-11