Merbau wood
Merbau is a hardwood. The Handbook prints the dry mechanical properties at 15% moisture content, not at 12%, so they are not ranked on the 12% Janka scale. Side hardness at 15% moisture is 1,500 lbf1 6,700 N2.
It moves about 0.16%3 across the width of a flat-sawn board for each 1% change in moisture content.
Key numbers
| Property | Merbau |
|---|---|
| Janka hardness, 15% MC | 1,500 lbf1; 6,700 N2 |
| Janka hardness, green | 1,380 lbf1 |
| Specific gravity, green volume basis | 0.641 |
| Bending strength (MOR), 15% MC | 16,800 psi1; 115,800 kPa2 |
| Stiffness (MOE), 15% MC | 2.23 × 106 psi1; 15,400 MPa2 |
| Shrinkage, green to oven-dry | radial 2.7%, tangential 4.6%, volumetric 7.8%4 |
| T/R ratio (tangential ÷ radial) | 1.70, calculated5 |
| Movement coefficients | CR 0.00092, calculated; CT 0.00158, calculated3 |
How much does it move?
A 10-inch flat-sawn merbau board going from 6% to 10% moisture content, the range the Handbook recommends for individual pieces of interior woodwork in most of the United States7, widens by 0.063 in6. A quartersawn board widens by 0.037 in6.
The coefficients apply from 6% to 14% moisture content8.
Try your own board in the wood movement calculator.
What it's used for
Freshly cut heartwood is yellowish to orange-brown and turns brown or dark red-brown on exposure. The texture is rather coarse, the grain is straight to interlocked or wavy, and the wood is rather difficult to saw, though it dresses smoothly in most operations and finishes well. It is used in furniture, fine joinery, turnery, cabinets, flooring, and musical instruments.9
Compare with
Questions
- Is merbau a hardwood?
- Yes. Merbau is a hardwood10. In the Handbook, hardwood means a broad-leaved angiosperm, not a wood that is necessarily hard. Specific gravity on a green volume basis is 0.641.
- What is the Janka hardness of merbau?
- At 15% moisture the Handbook prints 1,500 lbf1 (6,700 N2). There is no 12% figure, so merbau is not ranked with the 12% scale.
- How much does merbau shrink?
- From green to oven-dry, tangential shrinkage is 4.6% and radial shrinkage is 2.7%4. The T/R ratio is 1.70, calculated5.
References
- 1. USDA Wood Handbook (FPL-GTR-282), Table 5-5b, p. 5-23
- 2. USDA Wood Handbook (FPL-GTR-282), Table 5-5a, p. 5-19
- 3. Calculated with Wood Handbook Eq. 13-2 (p. 13-16) from Table 4-4 (p. 4-9)
- 4. USDA Wood Handbook (FPL-GTR-282), Table 4-4, p. 4-9
- 5. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-4, p. 4-9).
- 6. Calculated with Wood Handbook Eq. 13-3 (p. 13-16): 10 in × the coefficient × 4 percentage points. Tangential coefficient 0.00158; radial coefficient 0.00092.
- 7. USDA Wood Handbook (FPL-GTR-282), Table 13-2, p. 13-5
- 8. USDA Wood Handbook (FPL-GTR-282), ch. 13, p. 13-16
- 9. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-31
- 10. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-2