Chinese JoineryChinese Joinery
Wood

Mahogany (genuine, Swietenia) wood

Mahogany (genuine, Swietenia macrophylla) is a medium-soft hardwood2: 800 lbf1 on the Janka side-hardness test at 12% moisture, below black cherry (950 lbf4) and above yellow-poplar (540 lbf3).

It is flexible5, and it moves about 0.14%6 across the width of a flat-sawn board for each 1% change in moisture content.

Key numbers

PropertyTrue mahogany
Janka hardness, 12% MC800 lbf1; 3,600 N7
Janka hardness, green740 lbf1
Specific gravity, green volume basis0.451
Bending strength (MOR), 12% MC11,500 psi1; 79,300 kPa7
Stiffness (MOE), 12% MC1.5 × 106 psi1; 10,300 MPa7
Shrinkage, green to oven-dryradial 3%, tangential 4.1%, volumetric 7.8%8
T/R ratio (tangential ÷ radial)1.37, calculated9
Movement coefficientsCR 0.00102, calculated; CT 0.00141, calculated6

How hard is mahogany (genuine, swietenia)?

01,0002,0003,0004,000true mahogany 800 lbf

Ticks are the anchor woods, from eastern white pine to ipe; the scale is in lbf. See true mahogany on the Janka chart.

How much does it move?

A 10-inch flat-sawn true mahogany board going from 6% to 10% moisture content, the range the Handbook recommends for individual pieces of interior woodwork in most of the United States11, widens by 0.056 in10. A quartersawn board widens by 0.041 in10.

The coefficients apply from 6% to 14% moisture content12.

Try your own board in the wood movement calculator.

What it's used for

The heartwood varies from pale pink or salmon to dark reddish brown; the grain is generally straighter than that of African mahogany, though many patterns occur, and the texture is rather fine to coarse. The wood dries without much warp, is very easy to work, slices into fine veneer, and takes an excellent polish. It is used for fine furniture, cabinets, interior woodwork, boats, fancy veneers, musical instruments, paneling, turnery, and carving.13

Compare with

Questions

Is mahogany a hardwood?
Yes. Mahogany is a hardwood14. In the Handbook, hardwood means a broad-leaved angiosperm, not a wood that is necessarily hard. Specific gravity on a green volume basis is 0.451.
Is mahogany harder than black cherry?
Mahogany is softer than black cherry: 800 lbf1 versus 950 lbf4, both at 12% moisture.
How much does mahogany shrink?
From green to oven-dry, tangential shrinkage is 4.1% and radial shrinkage is 3%8. The T/R ratio is 1.37, calculated9.

References

  • 1. USDA Wood Handbook (FPL-GTR-282), Table 5-5b, p. 5-23
  • 2. Calculated from the 12% moisture Janka side-hardness values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 3. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-11
  • 4. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-9
  • 5. Calculated from the 12% moisture modulus of elasticity values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 6. Calculated with Wood Handbook Eq. 13-2 (p. 13-16) from Table 4-4 (p. 4-9)
  • 7. USDA Wood Handbook (FPL-GTR-282), Table 5-5a, p. 5-19
  • 8. USDA Wood Handbook (FPL-GTR-282), Table 4-4, p. 4-9
  • 9. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-4, p. 4-9).
  • 10. Calculated with Wood Handbook Eq. 13-3 (p. 13-16): 10 in × the coefficient × 4 percentage points. Tangential coefficient 0.00141; radial coefficient 0.00102.
  • 11. USDA Wood Handbook (FPL-GTR-282), Table 13-2, p. 13-5
  • 12. USDA Wood Handbook (FPL-GTR-282), ch. 13, p. 13-16
  • 13. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-29
  • 14. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-2