Larch (western larch) wood
Larch (western larch, Larix occidentalis) is a medium-soft softwood2: 830 lbf1 on the Janka side-hardness test at 12% moisture, below black cherry (950 lbf4) and well above yellow-poplar (540 lbf3).
It is moderately stiff5, and it moves about 0.32%6 across the width of a flat-sawn board for each 1% change in moisture content.
Key numbers
| Property | Western larch |
|---|---|
| Janka hardness, 12% MC | 830 lbf1; 3,700 N7 |
| Janka hardness, green | 510 lbf1 |
| Specific gravity, 12% MC volume basis | 0.521 |
| Bending strength (MOR), 12% MC | 13,000 psi1; 90,000 kPa7 |
| Stiffness (MOE), 12% MC | 1.87 × 106 psi1; 12,900 MPa7 |
| Shrinkage, green to oven-dry | radial 4.5%, tangential 9.1%, volumetric 14%8 |
| T/R ratio (tangential ÷ radial) | 2.02, calculated9 |
| Movement coefficients | CR 0.00155; CT 0.003236 |
How hard is larch (western larch)?
Ticks are the anchor woods, from eastern white pine to ipe; the scale is in lbf. See western larch on the Janka chart.
How much does it move?
A 10-inch flat-sawn western larch board going from 6% to 10% moisture content, the range the Handbook recommends for individual pieces of interior woodwork in most of the United States11, widens by 0.129 in10. A quartersawn board widens by 0.062 in10.
The coefficients apply from 6% to 14% moisture content12.
Try your own board in the wood movement calculator.
What it's used for
The heartwood is yellowish brown and the sapwood is yellowish white. The wood is usually straight grained and splits easily. It is used mainly for rough dimension, planks and boards, ties, and mine timbers, and some high-grade material is made into interior woodwork, flooring, sashes, and doors.13
Compare with
Questions
- Is larch a hardwood?
- No. Larch is a softwood14. Softwoods are conifers. The name is botanical, not a hardness ranking. Specific gravity on a 12% MC volume basis is 0.521.
- Is larch harder than black cherry?
- Larch is softer than black cherry: 830 lbf1 versus 950 lbf4, both at 12% moisture.
- How much does larch shrink?
- From green to oven-dry, tangential shrinkage is 9.1% and radial shrinkage is 4.5%8. The T/R ratio is 2.02, calculated9.
References
- 1. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-12
- 2. Calculated from the 12% moisture Janka side-hardness values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
- 3. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-11
- 4. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-9
- 5. Calculated from the 12% moisture modulus of elasticity values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
- 6. USDA Wood Handbook (FPL-GTR-282), Table 13-5, p. 13-17
- 7. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-7
- 8. USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8
- 9. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8).
- 10. Calculated with Wood Handbook Eq. 13-3 (p. 13-16): 10 in × the coefficient × 4 percentage points. Tangential coefficient 0.00323; radial coefficient 0.00155.
- 11. USDA Wood Handbook (FPL-GTR-282), Table 13-2, p. 13-5
- 12. USDA Wood Handbook (FPL-GTR-282), ch. 13, p. 13-16
- 13. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-13
- 14. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-2