Jatoba (courbaril) wood
Jatoba (courbaril, Hymenaea courbaril) is a very hard hardwood2: 2,350 lbf1 on the Janka side-hardness test at 12% moisture, above shagbark hickory (1,880 lbf3) and well below ipe (3,680 lbf4).
It is stiff5, and it moves about 0.30%6 across the width of a flat-sawn board for each 1% change in moisture content.
Key numbers
| Property | Courbaril |
|---|---|
| Janka hardness, 12% MC | 2,350 lbf1; 10,500 N7 |
| Janka hardness, green | 1,970 lbf1 |
| Specific gravity, green volume basis | 0.711 |
| Bending strength (MOR), 12% MC | 19,400 psi1; 133,800 kPa7 |
| Stiffness (MOE), 12% MC | 2.16 × 106 psi1; 14,900 MPa7 |
| Shrinkage, green to oven-dry | radial 4.5%, tangential 8.5%, volumetric 12.7%8 |
| T/R ratio (tangential ÷ radial) | 1.89, calculated9 |
| Movement coefficients | CR 0.00155, calculated; CT 0.003, calculated6 |
How hard is jatoba (courbaril)?
Ticks are the anchor woods, from eastern white pine to ipe; the scale is in lbf. See courbaril on the Janka chart.
How much does it move?
A 10-inch flat-sawn courbaril board going from 6% to 10% moisture content, the range the Handbook recommends for individual pieces of interior woodwork in most of the United States11, widens by 0.120 in10. A quartersawn board widens by 0.062 in10.
The coefficients apply from 6% to 14% moisture content12.
Try your own board in the wood movement calculator.
What it's used for
The sapwood is gray-white, and freshly cut heartwood is salmon red to orange-brown, becoming russet or reddish brown when dried, often with dark streaks. The texture is medium to rather coarse and the grain is mostly interlocked, so planing is somewhat difficult, though the surface can be machined smooth. It is used for tool handles, steam-bent parts, flooring, turnery, furniture, cabinetwork, and veneer.13
Compare with
Questions
- Is jatoba a hardwood?
- Yes. Jatoba is a hardwood14. In the Handbook, hardwood means a broad-leaved angiosperm, not a wood that is necessarily hard. Specific gravity on a green volume basis is 0.711.
- Is jatoba harder than shagbark hickory?
- Jatoba is harder than shagbark hickory: 2,350 lbf1 versus 1,880 lbf3, both at 12% moisture.
- How much does jatoba shrink?
- From green to oven-dry, tangential shrinkage is 8.5% and radial shrinkage is 4.5%8. The T/R ratio is 1.89, calculated9.
References
- 1. USDA Wood Handbook (FPL-GTR-282), Table 5-5b, p. 5-22
- 2. Calculated from the 12% moisture Janka side-hardness values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
- 3. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-10
- 4. USDA Wood Handbook (FPL-GTR-282), Table 5-5b, p. 5-23
- 5. Calculated from the 12% moisture modulus of elasticity values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
- 6. Calculated with Wood Handbook Eq. 13-2 (p. 13-16) from Table 4-4 (p. 4-9)
- 7. USDA Wood Handbook (FPL-GTR-282), Table 5-5a, p. 5-18
- 8. USDA Wood Handbook (FPL-GTR-282), Table 4-4, p. 4-9
- 9. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-4, p. 4-9).
- 10. Calculated with Wood Handbook Eq. 13-3 (p. 13-16): 10 in × the coefficient × 4 percentage points. Tangential coefficient 0.003; radial coefficient 0.00155.
- 11. USDA Wood Handbook (FPL-GTR-282), Table 13-2, p. 13-5
- 12. USDA Wood Handbook (FPL-GTR-282), ch. 13, p. 13-16
- 13. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-23
- 14. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-2