Chinese JoineryChinese Joinery
Wood

Jarrah wood

Jarrah is a hardwood, hard on the Janka scale2: 1,910 lbf1 on the Janka side-hardness test at 12% moisture, almost the same as shagbark hickory (1,880 lbf3) and well below ipe (3,680 lbf1).

It is moderately stiff4, and it moves about 0.40%5 across the width of a flat-sawn board for each 1% change in moisture content.

Key numbers

PropertyJarrah
Janka hardness, 12% MC1,910 lbf1; 8,500 N6
Janka hardness, green1,290 lbf1
Specific gravity, green volume basis0.671
Bending strength (MOR), 12% MC16,200 psi1; 111,700 kPa6
Stiffness (MOE), 12% MC1.88 × 106 psi1; 13,000 MPa6
Shrinkage, green to oven-dryradial 7.7%, tangential 11%, volumetric 18.7%7
T/R ratio (tangential ÷ radial)1.43, calculated8
Movement coefficientsCR 0.00271, calculated; CT 0.00396, calculated5

How hard is jarrah?

01,0002,0003,0004,000jarrah 1,910 lbf

Ticks are the anchor woods, from eastern white pine to ipe; the scale is in lbf. See jarrah on the Janka chart.

How much does it move?

A 10-inch flat-sawn jarrah board going from 6% to 10% moisture content, the range the Handbook recommends for individual pieces of interior woodwork in most of the United States10, widens by 0.158 in9. A quartersawn board widens by 0.108 in9.

The coefficients apply from 6% to 14% moisture content11.

Try your own board in the wood movement calculator.

What it's used for

The heartwood is a uniform pink to dark red, often turning a deep brownish red with age and exposure, and the pale sapwood is usually narrow in old trees. The texture is even and moderately coarse, the grain is frequently interlocked or wavy, and the wood is difficult to work because of its density and irregular grain. It is used for decking, marine timbers, flooring, railroad ties, and other heavy construction.12

Compare with

Questions

Is jarrah a hardwood?
Yes. Jarrah is a hardwood13. In the Handbook, hardwood means a broad-leaved angiosperm, not a wood that is necessarily hard. Specific gravity on a green volume basis is 0.671.
Is jarrah harder than shagbark hickory?
Jarrah is harder than shagbark hickory: 1,910 lbf1 versus 1,880 lbf3, both at 12% moisture.
How much does jarrah shrink?
From green to oven-dry, tangential shrinkage is 11% and radial shrinkage is 7.7%7. The T/R ratio is 1.43, calculated8.

References

  • 1. USDA Wood Handbook (FPL-GTR-282), Table 5-5b, p. 5-23
  • 2. Calculated from the 12% moisture Janka side-hardness values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 3. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-10
  • 4. Calculated from the 12% moisture modulus of elasticity values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 5. Calculated with Wood Handbook Eq. 13-2 (p. 13-16) from Table 4-4 (p. 4-9)
  • 6. USDA Wood Handbook (FPL-GTR-282), Table 5-5a, p. 5-19
  • 7. USDA Wood Handbook (FPL-GTR-282), Table 4-4, p. 4-9
  • 8. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-4, p. 4-9).
  • 9. Calculated with Wood Handbook Eq. 13-3 (p. 13-16): 10 in × the coefficient × 4 percentage points. Tangential coefficient 0.00396; radial coefficient 0.00271.
  • 10. USDA Wood Handbook (FPL-GTR-282), Table 13-2, p. 13-5
  • 11. USDA Wood Handbook (FPL-GTR-282), ch. 13, p. 13-16
  • 12. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-26
  • 13. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-2