Iroko wood
Iroko is a medium-hard hardwood2: 1,260 lbf1 on the Janka side-hardness test at 12% moisture, almost the same as northern red oak (1,290 lbf4) and above black walnut (1,010 lbf3).
It is flexible5, and it moves about 0.13%6 across the width of a flat-sawn board for each 1% change in moisture content.
Key numbers
| Property | Iroko |
|---|---|
| Janka hardness, 12% MC | 1,260 lbf1; 5,600 N7 |
| Janka hardness, green | 1,080 lbf1 |
| Specific gravity, green volume basis | 0.541 |
| Bending strength (MOR), 12% MC | 12,400 psi1; 85,500 kPa7 |
| Stiffness (MOE), 12% MC | 1.46 × 106 psi1; 10,100 MPa7 |
| Shrinkage, green to oven-dry | radial 2.8%, tangential 3.8%, volumetric 8.8%8 |
| T/R ratio (tangential ÷ radial) | 1.36, calculated9 |
| Movement coefficients | CR 0.00095, calculated; CT 0.0013, calculated6 |
How hard is iroko?
Ticks are the anchor woods, from eastern white pine to ipe; the scale is in lbf. See iroko on the Janka chart.
How much does it move?
A 10-inch flat-sawn iroko board going from 6% to 10% moisture content, the range the Handbook recommends for individual pieces of interior woodwork in most of the United States11, widens by 0.052 in10. A quartersawn board widens by 0.038 in10.
The coefficients apply from 6% to 14% moisture content12.
Try your own board in the wood movement calculator.
What it's used for
The heartwood varies from pale yellowish brown to dark chocolate brown, with light markings most conspicuous on flat-sawn faces, and the sapwood is yellowish white. The texture is medium to coarse, the grain is typically interlocked, and the wood works easily, though the grain can tear. Because of its color and durability it has been suggested as a substitute for teak, and it is used for boats, joinery, flooring, furniture, veneer, and cabinetwork.13
Compare with
Questions
- Is iroko a hardwood?
- Yes. Iroko is a hardwood14. In the Handbook, hardwood means a broad-leaved angiosperm, not a wood that is necessarily hard. Specific gravity on a green volume basis is 0.541.
- Is iroko harder than northern red oak?
- Iroko is softer than northern red oak: 1,260 lbf1 versus 1,290 lbf4, both at 12% moisture.
- How much does iroko shrink?
- From green to oven-dry, tangential shrinkage is 3.8% and radial shrinkage is 2.8%8. The T/R ratio is 1.36, calculated9.
References
- 1. USDA Wood Handbook (FPL-GTR-282), Table 5-5b, p. 5-23
- 2. Calculated from the 12% moisture Janka side-hardness values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
- 3. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-11
- 4. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-10
- 5. Calculated from the 12% moisture modulus of elasticity values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
- 6. Calculated with Wood Handbook Eq. 13-2 (p. 13-16) from Table 4-4 (p. 4-9)
- 7. USDA Wood Handbook (FPL-GTR-282), Table 5-5a, p. 5-19
- 8. USDA Wood Handbook (FPL-GTR-282), Table 4-4, p. 4-9
- 9. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-4, p. 4-9).
- 10. Calculated with Wood Handbook Eq. 13-3 (p. 13-16): 10 in × the coefficient × 4 percentage points. Tangential coefficient 0.0013; radial coefficient 0.00095.
- 11. USDA Wood Handbook (FPL-GTR-282), Table 13-2, p. 13-5
- 12. USDA Wood Handbook (FPL-GTR-282), ch. 13, p. 13-16
- 13. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-25
- 14. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-2