Chinese JoineryChinese Joinery
Wood

Indian rosewood wood

Indian rosewood is a very hard hardwood2: 3,170 lbf1 on the Janka side-hardness test at 12% moisture, below ipe (3,680 lbf4) and well above shagbark hickory (1,880 lbf3).

It is moderately stiff5, and it moves about 0.20%6 across the width of a flat-sawn board for each 1% change in moisture content.

Key numbers

PropertyIndian rosewood
Janka hardness, 12% MC3,170 lbf1; 14,100 N7
Janka hardness, green1,560 lbf1
Specific gravity, green volume basis0.751
Bending strength (MOR), 12% MC16,900 psi1; 116,500 kPa7
Stiffness (MOE), 12% MC1.78 × 106 psi1; 12,300 MPa7
Shrinkage, green to oven-dryradial 2.7%, tangential 5.8%, volumetric 8.5%8
T/R ratio (tangential ÷ radial)2.15, calculated9
Movement coefficientsCR 0.00092, calculated; CT 0.00201, calculated6

How hard is Indian rosewood?

01,0002,0003,0004,000Indian rosewood 3,170 lbf

Ticks are the anchor woods, from eastern white pine to ipe; the scale is in lbf. See Indian rosewood on the Janka chart.

How much does it move?

A 10-inch flat-sawn Indian rosewood board going from 6% to 10% moisture content, the range the Handbook recommends for individual pieces of interior woodwork in most of the United States11, widens by 0.080 in10. A quartersawn board widens by 0.037 in10.

The coefficients apply from 6% to 14% moisture content12.

Try your own board in the wood movement calculator.

What it's used for

The heartwood varies from golden brown to dark purplish brown with blackish streaks, and the narrow sapwood is yellowish. The texture is uniform and moderately coarse, and the wood is moderately hard to work with hand tools and turns well. In the United States it is used primarily as veneer for high-quality furniture and cabinetwork.13

Compare with

Questions

Is Indian rosewood a hardwood?
Yes. Indian rosewood is a hardwood14. In the Handbook, hardwood means a broad-leaved angiosperm, not a wood that is necessarily hard. Specific gravity on a green volume basis is 0.751.
Is Indian rosewood harder than ipe?
Indian rosewood is softer than ipe: 3,170 lbf1 versus 3,680 lbf4, both at 12% moisture.
How much does Indian rosewood shrink?
From green to oven-dry, tangential shrinkage is 5.8% and radial shrinkage is 2.7%8. The T/R ratio is 2.15, calculated9.

References

  • 1. USDA Wood Handbook (FPL-GTR-282), Table 5-5b, p. 5-24
  • 2. Calculated from the 12% moisture Janka side-hardness values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 3. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-10
  • 4. USDA Wood Handbook (FPL-GTR-282), Table 5-5b, p. 5-23
  • 5. Calculated from the 12% moisture modulus of elasticity values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 6. Calculated with Wood Handbook Eq. 13-2 (p. 13-16) from Table 4-4 (p. 4-9)
  • 7. USDA Wood Handbook (FPL-GTR-282), Table 5-5a, p. 5-20
  • 8. USDA Wood Handbook (FPL-GTR-282), Table 4-4, p. 4-9
  • 9. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-4, p. 4-9).
  • 10. Calculated with Wood Handbook Eq. 13-3 (p. 13-16): 10 in × the coefficient × 4 percentage points. Tangential coefficient 0.00201; radial coefficient 0.00092.
  • 11. USDA Wood Handbook (FPL-GTR-282), Table 13-2, p. 13-5
  • 12. USDA Wood Handbook (FPL-GTR-282), ch. 13, p. 13-16
  • 13. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-35
  • 14. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-2