Elm (American elm) wood

Elm (American elm, Ulmus americana) is a medium-soft hardwood2: 830 lbf1 on the Janka side-hardness test at 12% moisture, below black cherry (950 lbf1) and well above yellow-poplar (540 lbf3).

It is flexible4, and it moves about 0.34%5 across the width of a flat-sawn board for each 1% change in moisture content.

Key numbers

PropertyAmerican elm
Janka hardness, 12% MC830 lbf1; 3,700 N6
Janka hardness, green620 lbf1
Specific gravity, 12% MC volume basis0.51
Bending strength (MOR), 12% MC11,800 psi1; 81,000 kPa6
Stiffness (MOE), 12% MC1.34 × 106 psi1; 9,200 MPa6
Shrinkage, green to oven-dryradial 4.2%, tangential 9.5%, volumetric 14.6%7
T/R ratio (tangential ÷ radial)2.26, calculated8
Movement coefficientsCR 0.00144; CT 0.003385

How hard is elm (American elm)?

01,0002,0003,0004,000American elm 830 lbf

Ticks are the anchor woods, from eastern white pine to ipe; the scale is in lbf. See American elm on the Janka chart.

How much does it move?

A 10-inch flat-sawn American elm board going from 6% to 10% moisture content, the range the Handbook recommends for individual pieces of interior woodwork in most of the United States10, widens by 0.135 in9. A quartersawn board widens by 0.058 in9.

The coefficients apply from 6% to 14% moisture content11.

Try your own board in the wood movement calculator.

What it's used for

The sapwood is nearly white and the heartwood is light brown, often tinged with red. American elm is in the soft elm class, and elm has excellent bending qualities. Today, elm lumber and veneer are used mostly for furniture and decorative panels; the lumber was also used for boxes, baskets, crates, and slack cooperage.12

Compare with

Questions

Is elm a hardwood?
Yes. Elm is a hardwood13. In the Handbook, hardwood means a broad-leaved angiosperm, not a wood that is necessarily hard. Specific gravity on a 12% MC volume basis is 0.51.
Is elm harder than black cherry?
Elm is softer than black cherry: 830 lbf1 versus 950 lbf1, both at 12% moisture.
How much does elm shrink?
From green to oven-dry, tangential shrinkage is 9.5% and radial shrinkage is 4.2%7. The T/R ratio is 2.26, calculated8.

References

  • 1. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-9
  • 2. Calculated from the 12% moisture Janka side-hardness values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 3. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-11
  • 4. Calculated from the 12% moisture modulus of elasticity values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 5. USDA Wood Handbook (FPL-GTR-282), Table 13-5, p. 13-17
  • 6. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-4
  • 7. USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8
  • 8. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8).
  • 9. Calculated with Wood Handbook Eq. 13-3 (p. 13-16): 10 in × the coefficient × 4 percentage points. Tangential coefficient 0.00338; radial coefficient 0.00144.
  • 10. USDA Wood Handbook (FPL-GTR-282), Table 13-2, p. 13-5
  • 11. USDA Wood Handbook (FPL-GTR-282), ch. 13, p. 13-16
  • 12. USDA Wood Handbook (FPL-GTR-282), ch. 2, pp. 2-6–2-7
  • 13. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-2