Eastern hemlock wood
Eastern hemlock is a softwood, soft on the Janka scale2: 500 lbf1 on the Janka side-hardness test at 12% moisture, almost the same as yellow-poplar (540 lbf3) and above eastern white pine (380 lbf1).
It is flexible4, and it moves about 0.24%5 across the width of a flat-sawn board for each 1% change in moisture content.
Key numbers
| Property | Eastern hemlock |
|---|---|
| Janka hardness, 12% MC | 500 lbf1; 2,200 N6 |
| Janka hardness, green | 400 lbf1 |
| Specific gravity, 12% MC volume basis | 0.41 |
| Bending strength (MOR), 12% MC | 8,900 psi1; 61,000 kPa6 |
| Stiffness (MOE), 12% MC | 1.2 × 106 psi1; 8,300 MPa6 |
| Shrinkage, green to oven-dry | radial 3%, tangential 6.8%, volumetric 9.7%7 |
| T/R ratio (tangential ÷ radial) | 2.27, calculated8 |
| Movement coefficients | CR 0.00102; CT 0.002375 |
How hard is eastern hemlock?
Ticks are the anchor woods, from eastern white pine to ipe; the scale is in lbf. See eastern hemlock on the Janka chart.
How much does it move?
A 10-inch flat-sawn eastern hemlock board going from 6% to 10% moisture content, the range the Handbook recommends for individual pieces of interior woodwork in most of the United States10, widens by 0.095 in9. A quartersawn board widens by 0.041 in9.
The coefficients apply from 6% to 14% moisture content11.
Try your own board in the wood movement calculator.
What it's used for
The heartwood is pale brown with a reddish hue. The sapwood is not distinctly separated from the heartwood but may be lighter, and the wood is coarse and uneven in texture. It is used for lumber and pulpwood; the lumber goes into framing, sheathing, subflooring, roof boards, boxes, pallets, and crates.12
Compare with
Questions
- Is eastern hemlock a hardwood?
- No. Eastern hemlock is a softwood13. Softwoods are conifers. The name is botanical, not a hardness ranking. Specific gravity on a 12% MC volume basis is 0.41.
- Is eastern hemlock harder than yellow-poplar?
- Eastern hemlock is softer than yellow-poplar: 500 lbf1 versus 540 lbf3, both at 12% moisture.
- How much does eastern hemlock shrink?
- From green to oven-dry, tangential shrinkage is 6.8% and radial shrinkage is 3%7. The T/R ratio is 2.27, calculated8.
References
- 1. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-12
- 2. Calculated from the 12% moisture Janka side-hardness values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
- 3. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-11
- 4. Calculated from the 12% moisture modulus of elasticity values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
- 5. USDA Wood Handbook (FPL-GTR-282), Table 13-5, p. 13-17
- 6. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-7
- 7. USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8
- 8. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8).
- 9. Calculated with Wood Handbook Eq. 13-3 (p. 13-16): 10 in × the coefficient × 4 percentage points. Tangential coefficient 0.00237; radial coefficient 0.00102.
- 10. USDA Wood Handbook (FPL-GTR-282), Table 13-2, p. 13-5
- 11. USDA Wood Handbook (FPL-GTR-282), ch. 13, p. 13-16
- 12. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-12
- 13. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-2