Douglas-fir (coast, Pseudotsuga menziesii) is a medium-soft softwood2: 710 lbf1 on the Janka side-hardness test at 12% moisture, above yellow-poplar (540 lbf3) and below black cherry (950 lbf4).

It is moderately stiff5, and it moves about 0.27%6 across the width of a flat-sawn board for each 1% change in moisture content.

Key numbers

PropertyDouglas-fir (Coast)
Janka hardness, 12% MC710 lbf1; 3,200 N7
Janka hardness, green500 lbf1
Specific gravity, 12% MC volume basis0.481
Bending strength (MOR), 12% MC12,400 psi1; 85,000 kPa7
Stiffness (MOE), 12% MC1.95 × 106 psi1; 13,400 MPa7
Shrinkage, green to oven-dryradial 4.8%, tangential 7.6%, volumetric 12.4%8
T/R ratio (tangential ÷ radial)1.58, calculated9
Movement coefficientsCR 0.00165; CT 0.002676

How hard is Douglas-fir?

01,0002,0003,0004,000Douglas-fir (coast) 710 lbf

Ticks are the anchor woods, from eastern white pine to ipe; the scale is in lbf. See Douglas-fir (coast) on the Janka chart.

How much does it move?

A 10-inch flat-sawn Douglas-fir (coast) board going from 6% to 10% moisture content, the range the Handbook recommends for individual pieces of interior woodwork in most of the United States11, widens by 0.107 in10. A quartersawn board widens by 0.066 in10.

The coefficients apply from 6% to 14% moisture content12.

Try your own board in the wood movement calculator.

What it's used for

Young trees of moderate to rapid growth have reddish heartwood and are called red-fir. Very narrow-ringed heartwood of old-growth trees may be yellowish brown and is known as yellow-fir. The wood is used mostly for building and construction as lumber, piles, and plywood, and also for sashes, doors, millwork, boxes, pallets, and crates, with smaller amounts in flooring, furniture, boats, and tanks.13

Compare with

Questions

Is Douglas-fir a hardwood?
No. Douglas-fir is a softwood14. Softwoods are conifers. The name is botanical, not a hardness ranking. Specific gravity on a 12% MC volume basis is 0.481.
Is Douglas-fir harder than yellow-poplar?
Douglas-fir is harder than yellow-poplar: 710 lbf1 versus 540 lbf3, both at 12% moisture.
How much does Douglas-fir shrink?
From green to oven-dry, tangential shrinkage is 7.6% and radial shrinkage is 4.8%8. The T/R ratio is 1.58, calculated9.

References

  • 1. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-12
  • 2. Calculated from the 12% moisture Janka side-hardness values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 3. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-11
  • 4. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-9
  • 5. Calculated from the 12% moisture modulus of elasticity values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 6. USDA Wood Handbook (FPL-GTR-282), Table 13-5, p. 13-17
  • 7. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-7
  • 8. USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8
  • 9. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8).
  • 10. Calculated with Wood Handbook Eq. 13-3 (p. 13-16): 10 in × the coefficient × 4 percentage points. Tangential coefficient 0.00267; radial coefficient 0.00165.
  • 11. USDA Wood Handbook (FPL-GTR-282), Table 13-2, p. 13-5