Chinese JoineryChinese Joinery
Wood

Chestnut (American chestnut) wood

Chestnut (American chestnut, Castanea dentata) is a soft hardwood2: 540 lbf1 on the Janka side-hardness test at 12% moisture, above eastern white pine (380 lbf3) and well below black cherry (950 lbf1).

It is flexible4, and it moves about 0.23%5 across the width of a flat-sawn board for each 1% change in moisture content.

Key numbers

PropertyAmerican chestnut
Janka hardness, 12% MC540 lbf1; 2,400 N6
Janka hardness, green420 lbf1
Specific gravity, 12% MC volume basis0.431
Bending strength (MOR), 12% MC8,600 psi1; 59,000 kPa6
Stiffness (MOE), 12% MC1.23 × 106 psi1; 8,500 MPa6
Shrinkage, green to oven-dryradial 3.4%, tangential 6.7%, volumetric 11.6%7
T/R ratio (tangential ÷ radial)1.97, calculated8
Movement coefficientsCR 0.00116; CT 0.002345

How hard is chestnut (American chestnut)?

01,0002,0003,0004,000American chestnut 540 lbf

Ticks are the anchor woods, from eastern white pine to ipe; the scale is in lbf. See American chestnut on the Janka chart.

How much does it move?

A 10-inch flat-sawn American chestnut board going from 6% to 10% moisture content, the range the Handbook recommends for individual pieces of interior woodwork in most of the United States10, widens by 0.094 in9. A quartersawn board widens by 0.046 in9.

The coefficients apply from 6% to 14% moisture content11.

Try your own board in the wood movement calculator.

What it's used for

The heartwood is grayish brown or brown and darkens with age; the sapwood is very narrow and almost white. The wood is coarse in texture, dries well, and is easy to work with tools. It was once used for poles, railroad ties, furniture, caskets, boxes, and crates, and it now appears most often as wormy chestnut for paneling, interior woodwork, and picture frames.12

Compare with

Questions

Is chestnut a hardwood?
Yes. Chestnut is a hardwood13. In the Handbook, hardwood means a broad-leaved angiosperm, not a wood that is necessarily hard. Specific gravity on a 12% MC volume basis is 0.431.
Is chestnut harder than yellow-poplar?
Chestnut is the same hardness as yellow-poplar: 540 lbf1 versus 540 lbf14, both at 12% moisture.
How much does chestnut shrink?
From green to oven-dry, tangential shrinkage is 6.7% and radial shrinkage is 3.4%7. The T/R ratio is 1.97, calculated8.

References

  • 1. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-9
  • 2. Calculated from the 12% moisture Janka side-hardness values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 3. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-12
  • 4. Calculated from the 12% moisture modulus of elasticity values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 5. USDA Wood Handbook (FPL-GTR-282), Table 13-5, p. 13-17
  • 6. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-4
  • 7. USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8
  • 8. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8).
  • 9. Calculated with Wood Handbook Eq. 13-3 (p. 13-16): 10 in × the coefficient × 4 percentage points. Tangential coefficient 0.00234; radial coefficient 0.00116.
  • 10. USDA Wood Handbook (FPL-GTR-282), Table 13-2, p. 13-5
  • 11. USDA Wood Handbook (FPL-GTR-282), ch. 13, p. 13-16
  • 12. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-6
  • 13. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-2
  • 14. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-11