Cherry (black cherry) wood
Cherry (black cherry, Prunus serotina) is a medium-hard hardwood2: 950 lbf1 on the Janka side-hardness test at 12% moisture, almost the same as teak (1,000 lbf4) and well above yellow-poplar (540 lbf3).
It is flexible5, and it moves about 0.25%6 across the width of a flat-sawn board for each 1% change in moisture content.
Key numbers
| Property | Black cherry |
|---|---|
| Janka hardness, 12% MC | 950 lbf1; 4,200 N7 |
| Janka hardness, green | 660 lbf1 |
| Specific gravity, 12% MC volume basis | 0.51 |
| Bending strength (MOR), 12% MC | 12,300 psi1; 85,000 kPa7 |
| Stiffness (MOE), 12% MC | 1.49 × 106 psi1; 10,300 MPa7 |
| Shrinkage, green to oven-dry | radial 3.7%, tangential 7.1%, volumetric 11.5%8 |
| T/R ratio (tangential ÷ radial) | 1.92, calculated9 |
| Movement coefficients | CR 0.00126; CT 0.002486 |
How hard is cherry (black cherry)?
Ticks are the anchor woods, from eastern white pine to ipe; the scale is in lbf. See black cherry on the Janka chart.
How much does it move?
A 10-inch flat-sawn black cherry board going from 6% to 10% moisture content, the range the Handbook recommends for individual pieces of interior woodwork in most of the United States11, widens by 0.099 in10. A quartersawn board widens by 0.050 in10.
The coefficients apply from 6% to 14% moisture content12.
Try your own board in the wood movement calculator.
What it's used for
The heartwood varies from light to dark reddish brown and has a distinctive luster. The wood has a fairly uniform texture and very good machining properties, and it is very stable after drying. It is used principally for furniture, fine veneer panels, and architectural woodwork, and also for caskets, woodenware, novelties, and patterns.13
Compare with
Questions
- Is cherry a hardwood?
- Yes. Cherry is a hardwood14. In the Handbook, hardwood means a broad-leaved angiosperm, not a wood that is necessarily hard. Specific gravity on a 12% MC volume basis is 0.51.
- Is cherry harder than teak?
- Cherry is softer than teak: 950 lbf1 versus 1,000 lbf4, both at 12% moisture.
- How much does cherry shrink?
- From green to oven-dry, tangential shrinkage is 7.1% and radial shrinkage is 3.7%8. The T/R ratio is 1.92, calculated9.
References
- 1. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-9
- 2. Calculated from the 12% moisture Janka side-hardness values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
- 3. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-11
- 4. USDA Wood Handbook (FPL-GTR-282), Table 5-5b, p. 5-25
- 5. Calculated from the 12% moisture modulus of elasticity values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
- 6. USDA Wood Handbook (FPL-GTR-282), Table 13-5, p. 13-17
- 7. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-4
- 8. USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8
- 9. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8).
- 10. Calculated with Wood Handbook Eq. 13-3 (p. 13-16): 10 in × the coefficient × 4 percentage points. Tangential coefficient 0.00248; radial coefficient 0.00126.
- 11. USDA Wood Handbook (FPL-GTR-282), Table 13-2, p. 13-5
- 12. USDA Wood Handbook (FPL-GTR-282), ch. 13, p. 13-16
- 13. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-6
- 14. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-2