Chinese JoineryChinese Joinery
Wood

Brazilian rosewood wood

Brazilian rosewood is a very hard hardwood2: 2,720 lbf1 on the Janka side-hardness test at 12% moisture, above shagbark hickory (1,880 lbf3) and below ipe (3,680 lbf4).

It is moderately stiff5, and it moves about 0.16%6 across the width of a flat-sawn board for each 1% change in moisture content.

Key numbers

PropertyBrazilian rosewood
Janka hardness, 12% MC2,720 lbf1; 12,100 N7
Janka hardness, green2,440 lbf1
Specific gravity, green volume basis0.81
Bending strength (MOR), 12% MC19,000 psi1; 131,000 kPa7
Stiffness (MOE), 12% MC1.88 × 106 psi1; 13,000 MPa7
Shrinkage, green to oven-dryradial 2.9%, tangential 4.6%, volumetric 8.5%8
T/R ratio (tangential ÷ radial)1.59, calculated9
Movement coefficientsCR 0.00099, calculated; CT 0.00158, calculated6

How hard is Brazilian rosewood?

01,0002,0003,0004,000Brazilian rosewood 2,720 lbf

Ticks are the anchor woods, from eastern white pine to ipe; the scale is in lbf. See Brazilian rosewood on the Janka chart.

How much does it move?

A 10-inch flat-sawn Brazilian rosewood board going from 6% to 10% moisture content, the range the Handbook recommends for individual pieces of interior woodwork in most of the United States11, widens by 0.063 in10. A quartersawn board widens by 0.040 in10.

The coefficients apply from 6% to 14% moisture content12.

Try your own board in the wood movement calculator.

What it's used for

The heartwood runs through shades of brown, red, and violet, irregularly and conspicuously streaked with black, and it is sharply marked off from the white sapwood. The texture is coarse, the grain is generally straight, and the heartwood has an oily or waxy feel and a fragrant odor; the wood machines and veneers well. It is used primarily as veneer for decorative plywood, with limited solid stock for handles, brush backs, and fancy turnery.13

Compare with

Questions

Is Brazilian rosewood a hardwood?
Yes. Brazilian rosewood is a hardwood14. In the Handbook, hardwood means a broad-leaved angiosperm, not a wood that is necessarily hard. Specific gravity on a green volume basis is 0.81.
Is Brazilian rosewood harder than shagbark hickory?
Brazilian rosewood is harder than shagbark hickory: 2,720 lbf1 versus 1,880 lbf3, both at 12% moisture.
How much does Brazilian rosewood shrink?
From green to oven-dry, tangential shrinkage is 4.6% and radial shrinkage is 2.9%8. The T/R ratio is 1.59, calculated9.

References

  • 1. USDA Wood Handbook (FPL-GTR-282), Table 5-5b, p. 5-24
  • 2. Calculated from the 12% moisture Janka side-hardness values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 3. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-10
  • 4. USDA Wood Handbook (FPL-GTR-282), Table 5-5b, p. 5-23
  • 5. Calculated from the 12% moisture modulus of elasticity values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 6. Calculated with Wood Handbook Eq. 13-2 (p. 13-16) from Table 4-4 (p. 4-9)
  • 7. USDA Wood Handbook (FPL-GTR-282), Table 5-5a, p. 5-20
  • 8. USDA Wood Handbook (FPL-GTR-282), Table 4-4, p. 4-9
  • 9. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-4, p. 4-9).
  • 10. Calculated with Wood Handbook Eq. 13-3 (p. 13-16): 10 in × the coefficient × 4 percentage points. Tangential coefficient 0.00158; radial coefficient 0.00099.
  • 11. USDA Wood Handbook (FPL-GTR-282), Table 13-2, p. 13-5
  • 12. USDA Wood Handbook (FPL-GTR-282), ch. 13, p. 13-16
  • 13. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-35
  • 14. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-2