Chinese JoineryChinese Joinery
Wood

Beech (American beech) wood

Beech (American beech, Fagus grandifolia) is a medium-hard hardwood2: 1,300 lbf1 on the Janka side-hardness test at 12% moisture, almost the same as northern red oak (1,290 lbf3) and below white oak (1,360 lbf4).

It is moderately stiff5, and it moves about 0.43%6 across the width of a flat-sawn board for each 1% change in moisture content.

Key numbers

PropertyAmerican beech
Janka hardness, 12% MC1,300 lbf1; 5,800 N7
Janka hardness, green850 lbf1
Specific gravity, 12% MC volume basis0.641
Bending strength (MOR), 12% MC14,900 psi1; 103,000 kPa7
Stiffness (MOE), 12% MC1.72 × 106 psi1; 11,900 MPa7
Shrinkage, green to oven-dryradial 5.5%, tangential 11.9%, volumetric 17.2%8
T/R ratio (tangential ÷ radial)2.16, calculated9
Movement coefficientsCR 0.0019; CT 0.004316

How hard is beech (American beech)?

01,0002,0003,0004,000American beech 1,300 lbf

Ticks are the anchor woods, from eastern white pine to ipe; the scale is in lbf. See American beech on the Janka chart.

How much does it move?

A 10-inch flat-sawn American beech board going from 6% to 10% moisture content, the range the Handbook recommends for individual pieces of interior woodwork in most of the United States11, widens by 0.172 in10. A quartersawn board widens by 0.076 in10.

The coefficients apply from 6% to 14% moisture content12.

Try your own board in the wood movement calculator.

What it's used for

The wood ranges from nearly white sapwood to reddish-brown heartwood, sometimes without a clear line between them. It has little figure and a close, uniform texture; it machines smoothly, turns well, and is highly suitable for steam bending. Most beech is used for flooring, furniture, brush blocks, handles, veneer, woodenware, containers, and cooperage.13

Compare with

Questions

Is beech a hardwood?
Yes. Beech is a hardwood14. In the Handbook, hardwood means a broad-leaved angiosperm, not a wood that is necessarily hard. Specific gravity on a 12% MC volume basis is 0.641.
Is beech harder than northern red oak?
Beech is harder than northern red oak: 1,300 lbf1 versus 1,290 lbf3, both at 12% moisture.
How much does beech shrink?
From green to oven-dry, tangential shrinkage is 11.9% and radial shrinkage is 5.5%8. The T/R ratio is 2.16, calculated9.

References

  • 1. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-9
  • 2. Calculated from the 12% moisture Janka side-hardness values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 3. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-10
  • 4. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-11
  • 5. Calculated from the 12% moisture modulus of elasticity values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 6. USDA Wood Handbook (FPL-GTR-282), Table 13-5, p. 13-17
  • 7. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-4
  • 8. USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8
  • 9. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8).
  • 10. Calculated with Wood Handbook Eq. 13-3 (p. 13-16): 10 in × the coefficient × 4 percentage points. Tangential coefficient 0.00431; radial coefficient 0.0019.
  • 11. USDA Wood Handbook (FPL-GTR-282), Table 13-2, p. 13-5
  • 12. USDA Wood Handbook (FPL-GTR-282), ch. 13, p. 13-16
  • 13. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-5
  • 14. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-2