Basswood wood
Basswood (American basswood, Tilia americana) is a soft hardwood2: 410 lbf1 on the Janka side-hardness test at 12% moisture, almost the same as eastern white pine (380 lbf3) and below yellow-poplar (540 lbf4).
It is flexible5, and it moves about 0.33%6 across the width of a flat-sawn board for each 1% change in moisture content.
Key numbers
| Property | American basswood |
|---|---|
| Janka hardness, 12% MC | 410 lbf1; 1,800 N7 |
| Janka hardness, green | 250 lbf1 |
| Specific gravity, 12% MC volume basis | 0.371 |
| Bending strength (MOR), 12% MC | 8,700 psi1; 60,000 kPa7 |
| Stiffness (MOE), 12% MC | 1.46 × 106 psi1; 10,100 MPa7 |
| Shrinkage, green to oven-dry | radial 6.6%, tangential 9.3%, volumetric 15.8%8 |
| T/R ratio (tangential ÷ radial) | 1.41, calculated9 |
| Movement coefficients | CR 0.0023; CT 0.00336 |
How hard is basswood?
Ticks are the anchor woods, from eastern white pine to ipe; the scale is in lbf. See American basswood on the Janka chart.
How much does it move?
A 10-inch flat-sawn American basswood board going from 6% to 10% moisture content, the range the Handbook recommends for individual pieces of interior woodwork in most of the United States11, widens by 0.132 in10. A quartersawn board widens by 0.092 in10.
The coefficients apply from 6% to 14% moisture content12.
Try your own board in the wood movement calculator.
What it's used for
The heartwood is pale yellowish brown, sometimes with darker streaks, and the wide sapwood is creamy white or pale brown. Dry wood has no odor or taste; it has a fine, even texture, is straight grained and easy to work, and it seldom warps in use. Lumber is used for venetian blinds, sash and door frames, molding, woodenware, and boxes, and the wood is a favorite of carvers.13
Compare with
Questions
- Is basswood a hardwood?
- Yes. Basswood is a hardwood14. In the Handbook, hardwood means a broad-leaved angiosperm, not a wood that is necessarily hard. Specific gravity on a 12% MC volume basis is 0.371.
- Is basswood harder than eastern white pine?
- Basswood is harder than eastern white pine: 410 lbf1 versus 380 lbf3, both at 12% moisture.
- How much does basswood shrink?
- From green to oven-dry, tangential shrinkage is 9.3% and radial shrinkage is 6.6%8. The T/R ratio is 1.41, calculated9.
References
- 1. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-9
- 2. Calculated from the 12% moisture Janka side-hardness values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
- 3. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-12
- 4. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-11
- 5. Calculated from the 12% moisture modulus of elasticity values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
- 6. USDA Wood Handbook (FPL-GTR-282), Table 13-5, p. 13-17
- 7. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-4
- 8. USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8
- 9. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8).
- 10. Calculated with Wood Handbook Eq. 13-3 (p. 13-16): 10 in × the coefficient × 4 percentage points. Tangential coefficient 0.0033; radial coefficient 0.0023.
- 11. USDA Wood Handbook (FPL-GTR-282), Table 13-2, p. 13-5
- 12. USDA Wood Handbook (FPL-GTR-282), ch. 13, p. 13-16
- 13. USDA Wood Handbook (FPL-GTR-282), ch. 2, pp. 2-4–2-5
- 14. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-2