Balsa wood
Balsa is a hardwood. The Handbook does not print a 12% Janka hardness for it. Specific gravity 0.161, green volume basis.
It is flexible2, and it moves about 0.27%3 across the width of a flat-sawn board for each 1% change in moisture content.
Key numbers
| Property | Balsa |
|---|---|
| Specific gravity, green volume basis | 0.161 |
| Bending strength (MOR), 12% MC | 3,140 psi1; 21,600 kPa4 |
| Stiffness (MOE), 12% MC | 0.49 × 106 psi1; 3,400 MPa4 |
| Shrinkage, green to oven-dry | radial 3%, tangential 7.6%, volumetric 10.8%5 |
| T/R ratio (tangential ÷ radial) | 2.53, calculated6 |
| Movement coefficients | CR 0.00102, calculated; CT 0.00267, calculated3 |
How much does it move?
A 10-inch flat-sawn balsa board going from 6% to 10% moisture content, the range the Handbook recommends for individual pieces of interior woodwork in most of the United States8, widens by 0.107 in7. A quartersawn board widens by 0.041 in7.
The coefficients apply from 6% to 14% moisture content9.
Try your own board in the wood movement calculator.
What it's used for
The wood is nearly white or oatmeal colored, often with a yellowish or pinkish hue, and it has a velvety feel. It is the lightest and softest of the woods on the market. Because it is light and very porous, it is used for floats, rafts, corestock, insulation, cushioning, sound modifiers, models, and novelties.10
Compare with
Questions
- Is balsa a hardwood?
- Yes. Balsa is a hardwood11. In the Handbook, hardwood means a broad-leaved angiosperm, not a wood that is necessarily hard. Specific gravity on a green volume basis is 0.161.
- How strong is balsa in bending?
- Modulus of rupture at 12% moisture is 3,140 psi1 (21,600 kPa4).
- How much does balsa shrink?
- From green to oven-dry, tangential shrinkage is 7.6% and radial shrinkage is 3%5. The T/R ratio is 2.53, calculated6.
References
- 1. USDA Wood Handbook (FPL-GTR-282), Table 5-5b, p. 5-22
- 2. Calculated from the 12% moisture modulus of elasticity values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
- 3. Calculated with Wood Handbook Eq. 13-2 (p. 13-16) from Table 4-4 (p. 4-9)
- 4. USDA Wood Handbook (FPL-GTR-282), Table 5-5a, p. 5-18
- 5. USDA Wood Handbook (FPL-GTR-282), Table 4-4, p. 4-9
- 6. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-4, p. 4-9).
- 7. Calculated with Wood Handbook Eq. 13-3 (p. 13-16): 10 in × the coefficient × 4 percentage points. Tangential coefficient 0.00267; radial coefficient 0.00102.
- 8. USDA Wood Handbook (FPL-GTR-282), Table 13-2, p. 13-5
- 9. USDA Wood Handbook (FPL-GTR-282), ch. 13, p. 13-16
- 10. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-21