Chinese JoineryChinese Joinery
Wood

Ash (white ash) wood

Ash (white ash, Fraxinus americana) is a medium-hard hardwood2: 1,320 lbf1 on the Janka side-hardness test at 12% moisture, almost the same as northern red oak (1,290 lbf3) and almost the same as white oak (1,360 lbf4).

It is moderately stiff5, and it moves about 0.27%6 across the width of a flat-sawn board for each 1% change in moisture content.

Key numbers

PropertyWhite ash
Janka hardness, 12% MC1,320 lbf1; 5,900 N7
Janka hardness, green960 lbf1
Specific gravity, 12% MC volume basis0.61
Bending strength (MOR), 12% MC15,400 psi1; 106,000 kPa7
Stiffness (MOE), 12% MC1.74 × 106 psi1; 12,000 MPa7
Shrinkage, green to oven-dryradial 4.9%, tangential 7.8%, volumetric 13.3%8
T/R ratio (tangential ÷ radial)1.59, calculated9
Movement coefficientsCR 0.00169; CT 0.002746

How hard is ash (white ash)?

01,0002,0003,0004,000white ash 1,320 lbf

Ticks are the anchor woods, from eastern white pine to ipe; the scale is in lbf. See white ash on the Janka chart.

How much does it move?

A 10-inch flat-sawn white ash board going from 6% to 10% moisture content, the range the Handbook recommends for individual pieces of interior woodwork in most of the United States11, widens by 0.110 in10. A quartersawn board widens by 0.068 in10.

The coefficients apply from 6% to 14% moisture content12.

Try your own board in the wood movement calculator.

What it's used for

In the white ash group the heartwood is brown and the sapwood is light-colored or nearly white. American white ash is used for nonstriking tool handles, oars, baseball bats, and other sporting and athletic goods. The group is also used for decorative veneer, cabinets, furniture, flooring, millwork, and crates.13

Compare with

Questions

Is ash a hardwood?
Yes. Ash is a hardwood14. In the Handbook, hardwood means a broad-leaved angiosperm, not a wood that is necessarily hard. Specific gravity on a 12% MC volume basis is 0.61.
Is ash harder than northern red oak?
Ash is harder than northern red oak: 1,320 lbf1 versus 1,290 lbf3, both at 12% moisture.
How much does ash shrink?
From green to oven-dry, tangential shrinkage is 7.8% and radial shrinkage is 4.9%8. The T/R ratio is 1.59, calculated9.

References

  • 1. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-9
  • 2. Calculated from the 12% moisture Janka side-hardness values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 3. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-10
  • 4. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-11
  • 5. Calculated from the 12% moisture modulus of elasticity values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 6. USDA Wood Handbook (FPL-GTR-282), Table 13-5, p. 13-17
  • 7. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-4
  • 8. USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8
  • 9. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8).
  • 10. Calculated with Wood Handbook Eq. 13-3 (p. 13-16): 10 in × the coefficient × 4 percentage points. Tangential coefficient 0.00274; radial coefficient 0.00169.
  • 11. USDA Wood Handbook (FPL-GTR-282), Table 13-2, p. 13-5
  • 12. USDA Wood Handbook (FPL-GTR-282), ch. 13, p. 13-16
  • 13. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-4
  • 14. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-2