Chinese JoineryChinese Joinery
Wood

Alder (red alder) wood

Alder (red alder, Alnus rubra) is a medium-soft hardwood2: 590 lbf1 on the Janka side-hardness test at 12% moisture, almost the same as yellow-poplar (540 lbf3) and well below black cherry (950 lbf1).

It is flexible4, and it moves about 0.26%5 across the width of a flat-sawn board for each 1% change in moisture content.

Key numbers

PropertyRed alder
Janka hardness, 12% MC590 lbf1; 2,600 N6
Janka hardness, green440 lbf1
Specific gravity, 12% MC volume basis0.411
Bending strength (MOR), 12% MC9,800 psi1; 68,000 kPa6
Stiffness (MOE), 12% MC1.38 × 106 psi1; 9,500 MPa6
Shrinkage, green to oven-dryradial 4.4%, tangential 7.3%, volumetric 12.6%7
T/R ratio (tangential ÷ radial)1.66, calculated8
Movement coefficientsCR 0.00151; CT 0.002565

How hard is alder (red alder)?

01,0002,0003,0004,000red alder 590 lbf

Ticks are the anchor woods, from eastern white pine to ipe; the scale is in lbf. See red alder on the Janka chart.

How much does it move?

A 10-inch flat-sawn red alder board going from 6% to 10% moisture content, the range the Handbook recommends for individual pieces of interior woodwork in most of the United States10, widens by 0.102 in9. A quartersawn board widens by 0.060 in9.

The coefficients apply from 6% to 14% moisture content11.

Try your own board in the wood movement calculator.

What it's used for

The wood varies from almost white to pale pinkish brown, with no visible boundary between heartwood and sapwood. The principal use is furniture, and it is also used for sash and door panel stock and other millwork.12

Compare with

Questions

Is alder a hardwood?
Yes. Alder is a hardwood13. In the Handbook, hardwood means a broad-leaved angiosperm, not a wood that is necessarily hard. Specific gravity on a 12% MC volume basis is 0.411.
Is alder harder than yellow-poplar?
Alder is harder than yellow-poplar: 590 lbf1 versus 540 lbf3, both at 12% moisture.
How much does alder shrink?
From green to oven-dry, tangential shrinkage is 7.3% and radial shrinkage is 4.4%7. The T/R ratio is 1.66, calculated8.

References

  • 1. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-9
  • 2. Calculated from the 12% moisture Janka side-hardness values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 3. USDA Wood Handbook (FPL-GTR-282), Table 5-3b, p. 5-11
  • 4. Calculated from the 12% moisture modulus of elasticity values in the USDA Wood Handbook (FPL-GTR-282), Tables 5-3 and 5-5.
  • 5. USDA Wood Handbook (FPL-GTR-282), Table 13-5, p. 13-17
  • 6. USDA Wood Handbook (FPL-GTR-282), Table 5-3a, p. 5-4
  • 7. USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8
  • 8. Calculated from tangential shrinkage divided by radial shrinkage (USDA Wood Handbook (FPL-GTR-282), Table 4-3, p. 4-8).
  • 9. Calculated with Wood Handbook Eq. 13-3 (p. 13-16): 10 in × the coefficient × 4 percentage points. Tangential coefficient 0.00256; radial coefficient 0.00151.
  • 10. USDA Wood Handbook (FPL-GTR-282), Table 13-2, p. 13-5
  • 11. USDA Wood Handbook (FPL-GTR-282), ch. 13, p. 13-16
  • 12. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-3
  • 13. USDA Wood Handbook (FPL-GTR-282), ch. 2, p. 2-2