Chinese JoineryChinese Joinery
Lumber

Wood movement calculator

A 12 in. flat-sawn northern red oak board swells 0.146 in. going from 6% to 10% moisture content: for each 1% change in moisture, its width changes by 0.304% (coefficient 0.00304, Wood Handbook Table 13-5).

That is the tangential coefficient. A quartersawn board uses the radial coefficient, 0.00137. From 6% to 14% moisture content, the change in a dimension is the starting dimension times the coefficient times the change in moisture content. Flat-sawn width uses the tangential coefficient, CT. Quartersawn width uses the radial coefficient, CR.

The Handbook’s own example: a flat-grained white fir board 232 mm (9.15 in.) wide at 8% moisture content changes by 232 × 0.00245 × (11 − 8) = 1.705 mm (0.067 in.) at 11%, so it ends up 233.7 mm (9.217 in.) wide (Wood Handbook p. 13-16).

Where the list says “(calculated coefficient)”, Table 13-5 does not print a coefficient for that wood. The value is calculated with Eq. 13-2.

How to estimate a width change

  1. Multiply dimension, coefficient and moisture change. Multiply the starting dimension by the tangential coefficient for flat-sawn width, or the radial coefficient for quartersawn width, and by the difference between the end and start moisture contents.
Unit
Grain
Moisture

Handbook recommended installation range for individual pieces of interior woodwork (Table 13-2). Fig. 13-1 maps the areas. A button sets the start and end moisture contents to the limits of that range.

Change
12 × 0.00304 × (10 − 6) = 0.146 in. (3.71 mm). Nearest 1/64 in.: +9/64.
Final dimension
12.146 in. (308.51 mm)
Coefficient
CT 0.00304, Northern red oak. USDA Wood Handbook (FPL-GTR-282), Table 13-5, p. 13-17

A 12 in. flat-sawn northern red oak board swells 0.146 in. (3.71 mm) from 6% to 10% moisture content.

Commercial lumber is often not perfectly flat-sawn or quartersawn, so this method will probably overestimate width change and underestimate thickness change.

Questions

How much does wood expand with humidity?
Across the grain, the change is the starting dimension times the coefficient times the moisture change. A 12 in. flat-sawn northern red oak board from 6% to 10% changes by 12 × 0.00304 × 4 = 0.146 in. The tangential coefficient is 0.00304 and the radial coefficient is 0.00137 (Table 13-5). The coefficient is valid from 6% to 14% MC.
Does quartersawn wood move less?
For northern red oak the radial coefficient is 0.00137 and the tangential coefficient is 0.00304 (Table 13-5). Quartersawn width uses the radial coefficient, so a 12 in. board from 6% to 10% changes by 12 × 0.00137 × 4 = 0.066 in., against 0.146 in. flat-sawn.
What moisture content should furniture wood be?
Table 13-2 gives recommended moisture content at installation for interior woodwork, flooring, furniture and wood trim. In most of the United States the average is 8% and individual pieces are 6% to 10%. In the dry southwestern area the average is 6% and individual pieces are 4% to 9%. In the damp, warm coastal area the average is 11% and individual pieces are 8% to 13%. Fig. 13-1 maps those areas.

References